Physical Properties | Metric | English | Comments |
---|
Density | 0.689 g/cc @Temperature 371 °C | 0.0249 lb/in³ @Temperature 700 °F |
| 0.737 g/cc @Temperature 316 °C | 0.0266 lb/in³ @Temperature 600 °F |
| 0.769 g/cc @Temperature 260 °C | 0.0278 lb/in³ @Temperature 500 °F |
| 0.817 g/cc @Temperature 204 °C | 0.0295 lb/in³ @Temperature 400 °F |
| 0.865 g/cc @Temperature 149 °C | 0.0312 lb/in³ @Temperature 300 °F |
| 0.897 g/cc @Temperature 93.3 °C | 0.0324 lb/in³ @Temperature 200 °F |
| 0.945 g/cc @Temperature 37.8 °C | 0.0341 lb/in³ @Temperature 100 °F |
| 0.993 g/cc @Temperature -17.8 °C | 0.0359 lb/in³ @Temperature 0.000 °F |
Viscosity | 0.32 cP @Temperature 371 °C | 0.32 cP @Temperature 700 °F |
| 0.34 cP @Temperature 357 °C | 0.34 cP @Temperature 675 °F |
| 0.36 cP @Temperature 343 °C | 0.36 cP @Temperature 650 °F |
| 0.38 cP @Temperature 329 °C | 0.38 cP @Temperature 625 °F |
| 0.41 cP @Temperature 316 °C | 0.41 cP @Temperature 600 °F |
| 0.44 cP @Temperature 302 °C | 0.44 cP @Temperature 575 °F |
| 0.47 cP @Temperature 288 °C | 0.47 cP @Temperature 550 °F |
| 0.50 cP @Temperature 274 °C | 0.50 cP @Temperature 525 °F |
| 0.54 cP @Temperature 260 °C | 0.54 cP @Temperature 500 °F |
| 0.59 cP @Temperature 246 °C | 0.59 cP @Temperature 475 °F |
| 0.64 cP @Temperature 232 °C | 0.64 cP @Temperature 450 °F |
| 0.71 cP @Temperature 218 °C | 0.71 cP @Temperature 425 °F |
| 0.78 cP @Temperature 204 °C | 0.78 cP @Temperature 400 °F |
| 0.87 cP @Temperature 191 °C | 0.87 cP @Temperature 375 °F |
| 0.98 cP @Temperature 177 °C | 0.98 cP @Temperature 350 °F |
| 1.1 cP @Temperature 163 °C | 1.1 cP @Temperature 325 °F |
| 1.3 cP @Temperature 149 °C | 1.3 cP @Temperature 300 °F |
| 1.5 cP @Temperature 135 °C | 1.5 cP @Temperature 275 °F |
| 1.8 cP @Temperature 121 °C | 1.8 cP @Temperature 250 °F |
| 2.1 cP @Temperature 107 °C | 2.1 cP @Temperature 225 °F |
| 2.6 cP @Temperature 93.3 °C | 2.6 cP @Temperature 200 °F |
| 3.8 cP @Temperature 79.4 °C | 3.8 cP @Temperature 175 °F |
| 5.1 cP @Temperature 65.6 °C | 5.1 cP @Temperature 150 °F |
| 7.9 cP @Temperature 51.7 °C | 7.9 cP @Temperature 125 °F |
| 12 cP @Temperature 37.8 °C | 12 cP @Temperature 100 °F |
| 22 cP @Temperature 23.9 °C | 22 cP @Temperature 75.0 °F |
| 52 cP @Temperature 10.0 °C | 52 cP @Temperature 50.0 °F |
| 133 cP @Temperature -3.89 °C | 133 cP @Temperature 25.0 °F |
| 546 cP @Temperature -17.8 °C | 546 cP @Temperature 0.000 °F |
Molecular Weight | 240 g/mol | 240 g/mol |
Vapor Pressure | 0.00758 bar @Temperature 163 °C | 5.69 torr @Temperature 325 °F |
| 0.0338 bar @Temperature 204 °C | 25.4 torr @Temperature 400 °F |
| 0.117 bar @Temperature 246 °C | 87.8 torr @Temperature 475 °F |
| 0.345 bar @Temperature 288 °C | 259 torr @Temperature 550 °F |
| 0.896 bar @Temperature 329 °C | 672 torr @Temperature 625 °F |
| 2.00 bar @Temperature 371 °C | 1500 torr @Temperature 700 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 324 µm/m-°C | 180 µin/in-°F |
Specific Heat Capacity | 1.84 J/g-°C @Temperature -17.8 °C | 0.440 BTU/lb-°F @Temperature 0.000 °F |
| 1.97 J/g-°C @Temperature 37.8 °C | 0.470 BTU/lb-°F @Temperature 100 °F |
| 2.09 J/g-°C @Temperature 93.3 °C | 0.500 BTU/lb-°F @Temperature 200 °F |
| 2.22 J/g-°C @Temperature 149 °C | 0.530 BTU/lb-°F @Temperature 300 °F |
| 2.34 J/g-°C @Temperature 204 °C | 0.560 BTU/lb-°F @Temperature 400 °F |
| 2.47 J/g-°C @Temperature 260 °C | 0.590 BTU/lb-°F @Temperature 500 °F |
| 2.59 J/g-°C @Temperature 316 °C | 0.620 BTU/lb-°F @Temperature 600 °F |
| 2.72 J/g-°C @Temperature 371 °C | 0.650 BTU/lb-°F @Temperature 700 °F |
Thermal Conductivity | 0.0813 W/m-K @Temperature 371 °C | 0.564 BTU-in/hr-ft²-°F @Temperature 700 °F |
| 0.0916 W/m-K @Temperature 316 °C | 0.636 BTU-in/hr-ft²-°F @Temperature 600 °F |
| 0.0986 W/m-K @Temperature 260 °C | 0.684 BTU-in/hr-ft²-°F @Temperature 500 °F |
| 0.105 W/m-K @Temperature 204 °C | 0.732 BTU-in/hr-ft²-°F @Temperature 400 °F |
| 0.111 W/m-K @Temperature 149 °C | 0.768 BTU-in/hr-ft²-°F @Temperature 300 °F |
| 0.114 W/m-K @Temperature 93.3 °C | 0.792 BTU-in/hr-ft²-°F @Temperature 200 °F |
| 0.118 W/m-K @Temperature -17.8 °C | 0.816 BTU-in/hr-ft²-°F @Temperature 0.000 °F |
| 0.118 W/m-K @Temperature 37.8 °C | 0.816 BTU-in/hr-ft²-°F @Temperature 100 °F |
Maximum Service Temperature, Air | 343 °C | 650 °F |
| 357 °C | 675 °F |
| 371 °C | 700 °F |
Minimum Service Temperature, Air | -10.6 °C | 13.0 °F |
| 25.0 °C | 77.0 °F |
Pour Point | <= -34.4 °C | <= -30.0 °F |
Flash Point | >= 160 °C | >= 320 °F |
| >= 166 °C | >= 330 °F |
|
Descriptive Properties |
---|
Appearance | Almost Colorless |
Base | Alkylated Aromatic |
Odor | Slight |