MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 713.0-T5, Sand Cast
Categories: Metal; Nonferrous Metal; Aluminum Alloy; Aluminum Casting Alloy

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 713.0-T5; UNS A07130; AA713.0-T5; Al713.0-T5
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.81 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 60 - 90AA; Typical; 500 g load; 10 mm ball
Hardness, Knoop 98Estimated from Brinell Hardness.
Hardness, Vickers 85Estimated from Brinell Hardness.
Tensile Strength, Ultimate >= 32.0 ksiAA
Tensile Strength, Yield >= 22.0 ksi
@Strain 0.2 %
AA
Elongation at Break >= 3.0 %AA; in 2 in. (50 mm) or 4D
Tensile Modulus 71.0 GPaAluminum 770.0
Poissons Ratio 0.33Estimated from aluminum 770.0
Fatigue Strength 60.0 MPa
@# of Cycles 5.00e+8
Notch Status unknown, R.R. Moore Test
Machinability 90 %0-100 Scale (100=best)
Shear Modulus 26.5 GPaEstimated from aluminum 770.0
Shear Strength 180 MPa
Charpy Impact 3.40 JV-notch
Charpy Impact, Unnotched 16.3 J
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000570 ohm-cm
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 389 J/gTypical for cast aluminum
CTE, linear 24.1 µm/m-°C
@Temperature 20.0 - 100 °C
 26.3 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.963 J/g-°CTypical for cast aluminum
Thermal Conductivity 121 W/m-K
Melting Point 593 - 638 °C
Solidus 593 °C
Liquidus 638 °C
 
Processing PropertiesOriginal ValueComments
Melt Temperature 1100 - 1185 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 87.5 - 92.4 %As remainder
Chromium, Cr <= 0.35 %
Copper, Cu 0.40 - 1.0 %
Iron, Fe <= 1.1 %
Magnesium, Mg 0.20 - 0.50 %
Manganese, Mn <= 0.60 %
Nickel, Ni <= 0.15 %
Other, each <= 0.10 %
Other, total <= 0.25 %
Silicon, Si <= 0.25 %
Titanium, Ti <= 0.25 %
Zinc, Zn 7.0 - 8.0 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 713.0-F, Sand Cast
Aluminum 713.0-T5, Permanent Mold Cast
Aluminum 712.0-F, Sand Cast
713.1 Aluminum Composition Spec
Aluminum 710.0-T5, Sand Cast

MAC7130T5S / 10185

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.