MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

BASF Ultraform® H 2320 006 AT BK120 POM
Categories: Polymer; Thermoplastic; Acetal (Polyoxymethylene, POM)

Material Notes: Ultraform H 2320 006 AT BK120 is a pigmented black POM with high molecular weight for injection molding.

Applications: Typical applications include thick-walled articles.

Information provided by BASF.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.41 g/cc0.0509 lb/in³ISO 1183
Moisture Absorption 0.200 %0.200 %50% RH; ISO 62
Water Absorption at Saturation 0.90 %0.90 %ISO 62
Linear Mold Shrinkage, Flow 0.021 cm/cm0.021 in/inISO 294-4
Linear Mold Shrinkage, Transverse 0.021 cm/cm0.021 in/inISO 294-4
Melt Flow 2.9 g/10 min
@Load 2.16 kg,
Temperature 190 °C
2.9 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 62.0 MPa8990 psiISO 527
Elongation at Break 30 %30 %Nominal; ISO 527
Elongation at Yield 11 %11 %ISO 527
Tensile Modulus 2.60 GPa377 ksiISO 527
Izod Impact, Notched (ISO)  6.50 kJ/m²
@Temperature 23.0 °C
3.09 ft-lb/in²
@Temperature 73.4 °F
ISO 180
 7.00 kJ/m²
@Temperature -30.0 °C
3.33 ft-lb/in²
@Temperature -22.0 °F
ISO 180
Charpy Impact Unnotched  26.0 J/cm²
@Temperature -30.0 °C
124 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 27.0 J/cm²
@Temperature 23.0 °C
128 ft-lb/in²
@Temperature 73.4 °F
ISO 179
Charpy Impact, Notched  0.550 J/cm²
@Temperature -30.0 °C
2.62 ft-lb/in²
@Temperature -22.0 °F
ISO 179
 0.650 J/cm²
@Temperature 23.0 °C
3.09 ft-lb/in²
@Temperature 73.4 °F
ISO 179
Tensile Creep Modulus, 1000 hours 1300 MPa189000 psiISO 899
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 1.00e+11 ohm-cm1.00e+11 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohm1.00e+13 ohmIEC 60093
Dielectric Constant 3.8
@Frequency 1e+6 Hz
3.8
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.0050
@Frequency 1e+6 Hz
0.0050
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 120 µm/m-°C66.7 µin/in-°F
Melting Point 165 °C329 °FISO 3146
Deflection Temperature at 1.8 MPa (264 psi) 94.0 °C201 °FISO 75
 
Processing PropertiesMetricEnglishComments
Melt Temperature 190 - 230 °C374 - 446 °F
Mold Temperature 45.0 - 105 °C113 - 221 °Fcan be used where applicable
 80.0 - 90.0 °C176 - 194 °Frecommended
 60.0 - 120 °C140 - 248 °F
Drying Temperature 80.0 - 110 °C
@Time 7200 - 14400 sec
176 - 230 °F
@Time 2.00 - 4.00 hour
Moisture Content <= 0.15 %<= 0.15 %
Injection Pressure 3.45 - 6.89 MPa500 - 1000 psi

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PBASF8917 / 254875

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.