MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

SK Chemicals SKYGREEN® SF200 Copolyester
Categories: Polymer; Thermoplastic; Polyester, TP

Material Notes: SKYGREEN® SF200 is a Copolyester grade ideal for shrink film and labels on various packaging applications. SF200 offers excellent transparency, glossy appearance, and outstanding printability. It also has a high shrinkage rate and low shrink force. The low shrink force prevents the deformation of thin packagings.

Applications: Shrink film and label. Packaging. Attributes: Transparency. High TD shrink rate. Low MD shrink rate. Low shrink force.

Information provided by SK Chemicals

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.28 g/cc1.28 g/ccASTM D792
Linear Mold Shrinkage 0.0030 - 0.0060 cm/cm0.0030 - 0.0060 in/inASTM D955
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 27.0 MPa3920 psiISO 527
Tensile Strength, Yield 53.0 MPa7690 psiISO 527
Elongation at Break 250 %250 %ISO 527
Elongation at Yield 4.2 %4.2 %ISO 527
Flexural Strength 71.0 MPa10300 psiISO 178
Flexural Modulus 2.10 GPa305 ksiISO 178
Izod Impact, Notched (ISO) 15.7 kJ/m²7.47 ft-lb/in²ISO 180
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 69.0 °C156 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FISO 75
 
Optical PropertiesMetricEnglishComments
Haze <= 1.0 %<= 1.0 %ASTM D1003
UV Transmittance 90 %90 %ASTM D1003

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSK9901 / 291426

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.