MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Huber Martoxid® KMS-96 Calcined Aluminum Oxide
Categories: Ceramic; Oxide; Aluminum Oxide

Material Notes: Martoxid® KMS-96 calcined aluminum oxide is a feedstock ready to press for uniaxial and isostatic pressing for the production of oxide ceramic bodies such as grinding media, insulating and wear-resistant parts, etc., produced in Bergheim, Germany.

CAS No.: 1344-28-1

EC/EINECS No.: 215-691-6

Information provided by J.M. Huber Corporation

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.40 g/cc
@Pressure 100 MPa
Green Density
 3.80 g/cc
@Treatment Temp. 1600 °C,
Time 7200 sec
Fired Density
Bulk Density 1.20 g/cc
Moisture Absorption <= 0.300 %
Particle Size 170 µmmedian granule size
 
Mechanical PropertiesOriginal ValueComments
Hardness, Vickers 17 - 19[kN/mm²], HV2, Sintered product
Modulus of Elasticity 340 GPa
Flexural Strength >= 300 MPa4-point Method, Sintered product
Abrasion 0.10[%], Sand Blasting Method, Sintered product
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 35.0 kV/mmSintered product
 
Thermal PropertiesOriginal ValueComments
Shrinkage 16 %Upon sintering
 
Component Elements PropertiesOriginal ValueComments
CaO 1.3 %
Fe2O3 <= 0.10 %
Loss on Ignition(%) 3.6 %
MgO 0.70 %
Na2O <= 0.10 %
SiO2 1.9 %
 
Descriptive Properties
Al(OH)3 (%)96
FunctionalityReady-To-Press Granulating
Functionality: Mechanical hardnessWear Resistant Material
Market/Application: IndustrialCeramics

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

EHUBER805 / 300911

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.