MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Spartech PP5440 Glass Fiber Reinforced Homopolymer
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene with 40% Glass Fiber Filler

Material Notes: Provides the maximum strength and heat resistance among polypropylene compounds. Physical properties can approach those of more expensive engineering resins.

Information provided by Spartech

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.23 g/cc
@Temperature 22.8 °C
1.23 g/cc
@Temperature 73.0 °F
ASTM D792
Filler Content 40 %40 %
Linear Mold Shrinkage 0.0030 cm/cm0.0030 in/in0.125inch wall
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 89.6 MPa13000 psiASTM D638
Elongation at Break 2.0 %2.0 %ASTM D638
Elongation at Yield 1.0 %1.0 %ASTM D638
Flexural Strength 131 MPa19000 psiMax Load; ASTM D790
Flexural Modulus 5.52 GPa800 ksisecant; ASTM D790
 7.58 GPa1100 ksitangent; ASTM D790
Izod Impact, Notched 0.854 J/cm
@Temperature 22.8 °C
1.60 ft-lb/in
@Temperature 73.0 °F
ASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 157 °C315 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 149 °C300 °FASTM D648

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese SO.F.TER Polifor® QD 813 30% Glass Fiber Reinforced Self Extinguishing Polypropylene, Flame Resistant
Celanese SO.F.TER Polifor® 6 GF/30 30% Glass Fiber Reinforced Polypropylene
Asahi Kasei Thermylene® P7-40FG-0790 40% Glass Fiber Reinforced, Heat Stabilized Polypropylene
Asahi Kasei Thermylene® P6-40FG-0684 40% Glass Fiber Reinforced, Heat and UV Stabilized Polypropylene
Asahi Kasei Thermylene® P6-30FG-0709 30% Fiber Glass Reinforced, Heat Stabilized Polypropylene

PSPAR124 / 78746

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.