MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Multibase Multi-Flex® A 5001 LC Black TPE Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes:

Features:

  • Chemical Resistance, Good
  • Colorability, Good
  • Elasticity, High
  • Electrically Insulating
  • Flame Retardant
  • Flexibility, Good
  • Heat Stabilized
  • Ozone Resistant
  • Processability, Good
  • UV Resistance, Good
  • Weldable
  • Forms:

  • Pellets
  • Processing Method:

  • Extrusion
  • Information provided by Multibase

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Specific Gravity 1.06 g/cc1.06 g/ccASTM 792
    Melt Flow 2.0 g/10 min
    @Load 2.16 kg,
    Temperature 230 °C
    2.0 g/10 min
    @Load 4.76 lb,
    Temperature 446 °F
    ASTM D1238
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Shore A 464610 seconds; ASTM D2240
    Tensile Strength, Yield 5.52 MPa800 psiElastic; ASTM D412
    Elongation at Break 600 %600 %Elastic; ASTM D412
    Tear Strength 19.3 kN/m110 pliASTM D624
    Compression Set  13 %
    @Temperature 22.8 °C,
    Time 252000 sec
    13 %
    @Temperature 73.0 °F,
    Time 70.0 hour
    ASTM D395
     24 %
    @Temperature 70.0 °C,
    Time 252000 sec
    24 %
    @Temperature 158 °F,
    Time 70.0 hour
    ASTM D395
     
    Processing PropertiesMetricEnglishComments
    Die Temperature 204 °C400 °F
    Melt Temperature 191 - 204 °C375 - 400 °F

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    PMULTI021 / 53925

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.