MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Ovako C45 EN 10083-2:2006 Steel
Categories: Metal; Ferrous Metal; Alloy Steel; Carbon Steel; AISI 1000 Series Steel

Material Notes: General Information: Grade SB-C45 is one of our carbon steel grades with a narrowed chemical composition in order to reach a high hardenability and it is also fine grain treated with Al. Grade 047A is an ingot casted low alloyed steel. High hardness and high strength can be achieved after hardening thanks to the relatively high carbon content. The steel is suitable for various type of applications where high strength is needed.

Information provided by Ovako

Key Words: C43, C44, C45R - 1.1201, C45E - 1.1191, Ck45, St70-2, SAE 1045, 080A42, SS 1672, XC 48, C 45, S 45 C, GOST 45, AISI/SAE/ASTM 1045
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 7.80 g/cc0.282 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Modulus of Elasticity 210 GPa30500 ksi
Poissons Ratio 0.300.30
Shear Modulus 80.0 GPa11600 ksi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000200 - 0.00000250 ohm-cm0.00000200 - 0.00000250 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 12.0 µm/m-°C
@Temperature 20.0 - 300 °C
6.67 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.460 - 0.480 J/g-°C
@Temperature 50.0 - 100 °C
0.110 - 0.115 BTU/lb-°F
@Temperature 122 - 212 °F
Thermal Conductivity 40.0 - 45.0 W/m-K278 - 312 BTU-in/hr-ft²-°FAmbient temperature
Transformation Temperature 305 °C581 °FMS
 725 °C1340 °FAC1
 760 °C1400 °FAC3
 
Component Elements PropertiesMetricEnglishComments
Carbon, C 0.42 - 0.50 %0.42 - 0.50 %
Chromium, Cr <= 0.40 %<= 0.40 %
Iron, Fe 97.43 - 99.06 %97.43 - 99.06 %As Balance
Manganese, Mn 0.50 - 0.80 %0.50 - 0.80 %
Nickel, Ni <= 0.40 %<= 0.40 %
Phosphorus, P <= 0.030 %<= 0.030 %
Silicon, Si <= 0.40 %<= 0.40 %
Sulfur, S 0.020 - 0.040 %0.020 - 0.040 %
 
Descriptive Properties
WeldabilityCEV 0.65max
 Pcm 0.53max

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Ovako C45 SB1672 Steel
Ovako C45 SB1671 Steel
AISI 1045 Steel, cold drawn, 19-32 mm (0.75-1.25 in) round
Ovako C45 SB8673 Steel
Schmolz + Bickenbach Holder Block Plastic Mold Steel

NOVAKO393 / 234692

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.