MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Sulfur bearing Copper, UNS C14700, H04 Temper 6 mm rod
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Good to excellent corrosion resistance. Excellent hot and cold workability; good forgeability. Fabricated by coining, coppersmithing, drawing and upsetting, hot forging and pressing, spinning, swaging, stamping.

Applications: screw machine products and parts requiring high conductivity, extensive machining, corrosion resistance, copper color, or a combination of these: electrical connectors, motor and switch components, plumbing fittings, cold headed and machined parts, cold forgings, furnace-brazed articles, screws, soldering coppers, rivets and welding torch tips.

Test specimen: rod - 6mm diameter.

Key Words: C111, ISO CuSP, CEN CW114C
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.94 g/cc0.323 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B 5454
Tensile Strength, Ultimate 365 MPa52900 psi
Tensile Strength, Yield 340 MPa
@Strain 0.5 %
49300 psi
@Strain 0.5 %
Elongation at Break 10 %10 %In 50 mm
Modulus of Elasticity 115 GPa16700 ksi
Poissons Ratio 0.310.31Calculated
Machinability 85 %85 %UNS C36000 (free-cutting brass) = 100%
Forgeability 65 %65 %
Shear Modulus 44.0 GPa6380 ksi
Shear Strength 200 MPa29000 psi
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.00000181 ohm-cm
@Temperature 20.0 °C
0.00000181 ohm-cm
@Temperature 68.0 °F
 
Thermal PropertiesMetricEnglishComments
CTE, linear  17.0 µm/m-°C
@Temperature 20.0 - 100 °C
9.44 µin/in-°F
@Temperature 68.0 - 212 °F
 17.3 µm/m-°C
@Temperature 20.0 - 200 °C
9.61 µin/in-°F
@Temperature 68.0 - 392 °F
 17.7 µm/m-°C
@Temperature 20.0 - 300 °C
9.83 µin/in-°F
@Temperature 68.0 - 572 °F
Specific Heat Capacity 0.385 J/g-°C0.0920 BTU/lb-°F
Thermal Conductivity 374 W/m-K
@Temperature 20.0 °C
2600 BTU-in/hr-ft²-°F
@Temperature 68.0 °F
Melting Point 1067 - 1076 °C1953 - 1969 °F
Solidus 1067 °C1953 °F
Liquidus 1076 °C1969 °F
Annealing Point 427 - 649 °C800 - 1200 °F
 
Processing PropertiesMetricEnglishComments
Annealing Temperature 425 - 650 °C797 - 1200 °F
Hot-Working Temperature 750 - 875 °C1380 - 1610 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu 99.4 - 99.8 %99.4 - 99.8 %includes Ag
Other, total <= 0.10 %<= 0.10 %
Sulfur, S 0.20 - 0.50 %0.20 - 0.50 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Phosphorus deoxidized tellurium bearing Copper, UNS C14500, H04 Temper 6 mm rod
Leaded Copper, UNS C18700, H04 Temper 6 mm rod
Free-Cutting Brass, UNS C36000, H02 (Cold Drawn 25%) Temper 6 mm rod
Oxygen-free Copper (OF), UNS C10200, H02 Temper, flat products
Oxygen-free Copper (OF), UNS C10200, H04 Temper, flat products

MC14700b5 / 10629

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.