MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metalmen Sales

(Viewing data as-entered. Click here to return)
Aluminum 1145-H18
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 1000 Series Aluminum

Material Notes: Data points with the AA note have been provided by the Aluminum Association, Inc. and are NOT FOR DESIGN.

Composition Notes:
The aluminum content for unalloyed aluminum not made by a refining process is the difference between 100.00 percent and the sum of all other analyzed metallic elements present in amounts of 0.010 percent of more each, expressed to the second decimal before determining the sum. For alloys and unalloyed aluminum not made by a refining process, when the specified maximum limit is 0.XX, an observed value or a calculated value greater than 0.005 but less than 0.010% is rounded off and shown as " less than 0.01%".
Composition information provided by the Aluminum Association and is not for design.

Key Words: Aluminium 1145-H18; UNS A91145; Government QQ-A-1876; ASTM B 373; AA1145-H18; Al1145-H18
Vendors: Visit metalmen for your metals needs. Products include special chemistry, tight tolerances, custom tempers, odd dimensions/forms, and small quantities. Phone 1-800-767-9494.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 2.70 g/ccAA; Typical
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 39500 kg load with 10 mm ball. Calculated value.
Tensile Strength, Ultimate 145 MPa
Tensile Strength, Yield 115 MPa
Elongation at Break 5.0 %
@Thickness 1.60 mm
In 5 cm
Tensile Modulus 69.0 GPaCompressive Modulus is about 2% higher
Poissons Ratio 0.33
Shear Modulus 26.0 GPaCalculated
Shear Strength 85.0 MPaCalculated value.
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.00000290 ohm-cm
 
Thermal PropertiesOriginal ValueComments
Heat of Fusion 390 J/g
CTE, linear 21.8 µm/m-°C
@Temperature -50.0 - 20.0 °C
 23.6 µm/m-°C
@Temperature 20.0 - 100 °C
 24.5 µm/m-°C
@Temperature 20.0 - 200 °C
 25.5 µm/m-°C
@Temperature 20.0 - 300 °C
Specific Heat Capacity 0.904 J/g-°C
Thermal Conductivity 227 W/m-K
Melting Point 646 - 657 °C
Solidus 646 °C
Liquidus 657 °C
 
Optical PropertiesOriginal ValueComments
Emissivity (0-1) 0.040At 9.3 micron wavelength
Reflection Coefficient, Visible (0-1) 0.960.3-10 micron wavelength
 
Processing PropertiesOriginal ValueComments
Annealing Temperature 650 °F
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al >= 99.45 %Specified
Copper, Cu <= 0.05 %
Magnesium, Mg <= 0.05 %
Manganese, Mn <= 0.05 %
Other, each <= 0.03 %
Si+Fe <= 0.55 %
Titanium, Ti <= 0.03 %
Vanadium, V <= 0.05 %
Zinc, Zn <= 0.05 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aluminum 1145-O
Aluminum 1050-H14
Aluminum 1180-H18
Aluminum 1100-O
Aluminum 1050-H18

MA1145H18 / 8760

Metalmen Sales

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.