MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Teknor Apex Sinvicomp SZF6208 Flexible Polyvinyl Chloride
Categories: Polymer; Thermoplastic; Vinyl (PVC); PVC, Flexible Grade

Material Notes: Sinvicomp SSZ3709M is a wire & cable polyvinylchloride compound available in pellet form. It provides good performance for jacketing of cables.

Availability: Asia Pacific

Features: Low Temperature Resistance

Uses: Wire Jacketing

Agency Rating: UL 1581

RoHS Compliant:RoHS Compliant

Form: Pellets

Processing Method: Extrusion

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.35 g/cc0.0488 lb/in³ASTM D792
Deformation 30 %
@Temperature 120 °C,
Time 3600 sec
30 %
@Temperature 248 °F,
Time 1.00 hour
BS 6469
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A 7878ASTM D2240
Tensile Strength, Yield 16.0 MPa2320 psiASTM D638
 17.6 MPa
@Treatment Temp. 113 °C,
Time 605000 sec
2550 psi
@Treatment Temp. 235 °F,
Time 168 hour
Change after Aging in Air Oven; UL 1581
Elongation at Break 300 %300 %ASTM D638
 345 %
@Treatment Temp. 113 °C,
Time 605000 sec
345 %
@Treatment Temp. 235 °F,
Time 168 hour
Change after Aging in Air Oven; UL 1581
 
Thermal PropertiesMetricEnglishComments
Brittleness Temperature -36.0 °C-32.8 °FASTM D746
Oxygen Index 30 %30 %ASTM D2863
 
Processing PropertiesMetricEnglishComments
Processing Temperature 160 - 170 °C320 - 338 °FCompression zone
 170 - 175 °C338 - 347 °FMixing zone
Feed Temperature 150 °C302 °F
Nozzle Temperature 175 °C347 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1588 / 238079

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.