MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

BASF Ultramid® B3S Q661 PA6 (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, Unreinforced

Material Notes: Ultramid B3S Q661 is a general purpose, PA6 resin for injection molding.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.13 g/cc0.0408 lb/in³ISO 1183
Relative Viscosity 2.7 cP2.7 cPISO Test; 96 % SAV
Viscosity Number 150 cm³/g1.50 dl/g
Melt Flow 145 g/10 min
@Load 5.00 kg,
Temperature 275 °C
145 g/10 min
@Load 11.0 lb,
Temperature 527 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 79.0 MPa11500 psi50mm/min; ISO 527
 79.0 MPa11500 psi2 in/min; ASTM Test
Elongation at Break 4.2 %4.2 %2 in/min; ASTM Test
Elongation at Yield 4.2 %4.2 %50mm/min; ISO 527
Tensile Modulus 1.107 GPa160.6 ksi1mm/min; ISO 527
Flexural Modulus 2.74 GPa397 ksiASTM Test
Izod Impact, Notched 0.530 J/cm
@Thickness 3.17 mm
0.993 ft-lb/in
@Thickness 0.125 in
ASTM Test
 
Thermal PropertiesMetricEnglishComments
Melting Point 215 °C419 °FASTM Test
 220 °C428 °F10 K/min
Deflection Temperature at 0.46 MPa (66 psi) 180 °C356 °FASTM Test
 180 °C356 °FISO 75
Deflection Temperature at 1.8 MPa (264 psi) 76.0 °C169 °FASTM Test
 76.0 °C169 °FISO 75
 
Descriptive Properties
ColorNatural
Commercial StatusActive America
Impact ModifiedNo
Primary Processing TechniqueInjection Molding

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
BASF Ultramid® B3S HP PA6 (Dry)
BASF Ultramid® B3S BK00464 PA6 (Dry)
BASF Ultramid® B3S HP PA6 (Conditioned)
BASF Ultramid® B3S BK00464 PA6 (Conditioned)
ExxonMobil Santoprene® 101-64 Thermoplastic Elastomer

PBASF9328 / 85092

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.