MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
Eneos N241 Nitrile Rubber
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Characteristics: Low mold fouling

Application: Oil seal, gasket, diaphragm, hoses.

ENEOS has acquired the elastomer product lines from JSR Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 0.960 g/cc
Mooney Viscosity 56
@Temperature 100 °C
ML1+4
 64
@Temperature 100 °C
ML1+4, Compound (non-vulcanized)
 39
@Temperature 125 °C,
Time 54000 sec
Scorch Test, ML1, Compound (non-vulcanized)
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 70
 70Compound (vulcanized)
 54
@Temperature 40.0 °C,
Time 173000 sec
Fuel Oil B, Compound (non-vulcanized)
 55
@Temperature 120 °C,
Time 252000 sec
IRM903, Compound (vulcanized)
 67
@Temperature 120 °C,
Time 252000 sec
IRM901, Compound (vulcanized)
 74
@Temperature 120 °C,
Time 252000 sec
Air heat Aging, Compound (non-vulcanized)
Tensile Strength 19.7 MPa
 19.7 MPaCompound (vulcanized)
 8.077 MPa
@Temperature 40.0 °C,
Time 173000 sec
Fuel Oil B, Compound (non-vulcanized)
 15.563 MPa
@Temperature 120 °C,
Time 252000 sec
IRM903, Compound (vulcanized)
 20.882 MPa
@Temperature 120 °C,
Time 252000 sec
IRM901, Compound (vulcanized)
 22.261 MPa
@Temperature 120 °C,
Time 252000 sec
Air heat Aging, Compound (non-vulcanized)
Elongation at Break 400 %
 400 %Compound (vulcanized)
 188 %
@Temperature 40.0 °C,
Time 173000 sec
Fuel Oil B, Compound (non-vulcanized)
 308 %
@Temperature 120 °C,
Time 252000 sec
Air heat Aging, Compound (non-vulcanized)
 312 %
@Temperature 120 °C,
Time 252000 sec
IRM901, Compound (vulcanized)
 312 %
@Temperature 120 °C,
Time 252000 sec
IRM903, Compound (vulcanized)
100% Modulus 3.40 MPaCompound (vulcanized)
300% Modulus 15.3 MPa
 15.3 MPaCompound (vulcanized)
Resilience 48[%], Rebound, Compound (vulcanized)
Tear Strength 49.0 kN/mCompound (vulcanized)
Compression Set 14 %
@Temperature 100 °C,
Time 252000 sec
Compound (vulcanized)
 21 %
@Temperature 120 °C,
Time 252000 sec
Compound (vulcanized)
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -39.0 °C
 
Descriptive Properties
Acrylonitrile Content (%)29
Delta;V100 (%)0IRM901 70 hrs at 120°C, Compound (vulcanized)
 2Distilled Water 70 hr at 40°C, Compound (non-vulcanized)
 23IRM903 70 hrs at 120°C, Compound (vulcanized)
 43Fuel Oil B 48 hrs at 40°C, Compound (non-vulcanized)
 73Fuel Oil C 48 hrs at 40°C, Compound (non-vulcanized)
 95Fuel Oil C/Ethanol 48 hrs at 40°C, Compound (non-vulcanized)
Extrusion Test355 cc/min80°C, 25 rpm, Extrusion Volume
 363 cm/min80°C, 25 rpm, Extrusion Length
 9680°C, 25 rpm, Die Swell %
Flex Test15Occurrence(Thousand Times)
 3Growth 2 to 15 mm (Thousand Times)
Flow Rate70Q×104, 80°C, 100 kg, Kokahiki Flow tester
JSR Mold Curast Test 160°C, Minutes2tc(10)
 5tc(90)
Low-Temperature Torsion Test-31°Ct10
 -36°Ct100
Mill Contraction 50°C (%)44
Ozone Degradability TestC-3Static 20% Elongation, 50 ppm 5 Hours at 40°C
 C-3Dynamic 0 to 20% Elongation, 50 ppm 5 Hours at 40°C
Product formBale
Product StainSS

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PJSRC8067 / 295383

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.