MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Celanese Hytrel® 4053FG NC010 TPC-ET
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: 40 Shore D High Performance Polyester Elastomer Developed for Food Contact Applications

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.16 g/cc0.0419 lb/in³ISO 1183
Melt Density 1.02 g/cc
@Temperature 180 °C
0.0368 lb/in³
@Temperature 356 °F
Water Absorption 0.70 %
@Thickness 2.00 mm
0.70 %
@Thickness 0.0787 in
Sim. to ISO 62
Moisture Absorption 0.200 %
@Thickness 2.00 mm
0.200 %
@Thickness 0.0787 in
Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0020 cm/cm0.0020 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.0040 cm/cm0.0040 in/inISO 294-4, 2577
Melt Flow  5.0 g/10 min
@Load 2.16 kg,
Temperature 190 °C
5.0 g/10 min
@Load 4.76 lb,
Temperature 374 °F
cm³/10min Volumetric; ISO 1133
 5.3 g/10 min
@Load 2.16 kg,
Temperature 190 °C
5.3 g/10 min
@Load 4.76 lb,
Temperature 374 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 383815s; ISO 48-4
Tensile Stress at Strain  2.40 MPa
@Strain 5.0 %
348 psi
@Strain 5.0 %
1BA specimen at 50mm/min; ISO 527-1/-2
 4.40 MPa
@Strain 10 %
638 psi
@Strain 10 %
ISO 527-1/-2
 7.30 MPa
@Strain 50 %
1060 psi
@Strain 50 %
ISO 527-1/-2
Tensile Modulus 0.0560 GPa8.12 ksiISO 527-1/-2
Poissons Ratio 0.500.50
Charpy Impact Unnotched  NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eU
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eU
Charpy Impact, Notched  NB
@Temperature -40.0 °C
NB
@Temperature -40.0 °F
ISO 179/1eA
 NB
@Temperature -30.0 °C
NB
@Temperature -22.0 °F
ISO 179/1eA
 NB
@Temperature 23.0 °C
NB
@Temperature 73.4 °F
ISO 179/1eA
Tensile Impact Strength 230 kJ/m²
@Temperature 23.0 °C
109 ft-lb/in²
@Temperature 73.4 °F
Notched; ISO 8256/1
Tensile Creep Modulus, 1 hour 50.0 MPa7250 psi1h; ISO 899-1
Tensile Creep Modulus, 1000 hours 40.0 MPa5800 psi1000h; ISO 899-1
Tear Strength 110 kN/m628 pliparallel; ISO 34-1
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 7.00e+12 ohm-cm7.00e+12 ohm-cmIEC 62631-3-1
Surface Resistance 2.00e+14 ohm2.00e+14 ohmIEC 62631-3-2
Dielectric Constant  4.7
@Frequency 1e+6 Hz
4.7
@Frequency 1e+6 Hz
IEC 62631-2-1
 5.2
@Frequency 100 Hz
5.2
@Frequency 100 Hz
IEC 62631-2-1
Dielectric Strength 18.0 kV/mm457 kV/inIEC 60243-1
Dissipation Factor  0.011
@Frequency 100 Hz
0.011
@Frequency 100 Hz
IEC 62631-2-1
 0.0525
@Frequency 1e+6 Hz
0.0525
@Frequency 1e+6 Hz
IEC 62631-2-1
Comparative Tracking Index 600 V600 VIEC 60112
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 220 µm/m-°C122 µin/in-°FISO 11359-1/-2
CTE, linear, Transverse to Flow 220 µm/m-°C122 µin/in-°FISO 11359-1/-2
Melting Point 150 °C302 °F10°C/min; ISO 11357-1/-3
Glass Transition Temp, Tg -50.0 °C-58.0 °F10°C/min; ISO 11357-1/-2
Flammability, UL94 HB
@Thickness 1.50 mm
HB
@Thickness 0.0591 in
IEC 60695-11-10
Oxygen Index 20 %20 %ISO 4589-1/-2
 
Processing PropertiesMetricEnglishComments
Melt Temperature 170 °C338 °FOptimum, Extrusion
 165 - 180 °C329 - 356 °FRange, Extrusion
 170 - 190 °C338 - 374 °FRange, Injection
 180 °C356 °FOptimum, Injection
Mold Temperature 30.0 - 40.0 °C86.0 - 104 °FInjection
 40.0 °C104 °FOptimum, Injection
Drying Temperature 80.0 °C176 °FInjection
 70.0 - 90.0 °C158 - 194 °FExtrusion
Dry Time 2.00 - 3.00 hour2.00 - 3.00 hourExtrusion, Dehumidified Dryer
 2.00 - 3.00 hour2.00 - 3.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.060 %<= 0.060 %Extrusion
 <= 0.080 %<= 0.080 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
Eff. thermal diffusivity (m²/s)5.44E-08
FMVSS ClassSEISO 3795 (FMVSS 302)
Part Marking Code>TPC-ET<ISO 11469
PolymerTPC
Resin IdentificationTPC-ETISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Hytrel® 3046 NC010 TPC-ET
Celanese Hytrel® 3078 TPC-ET
Celanese Hytrel® 21UV TPC-ET
Celanese Hytrel® 4068 TPC-ET
Celanese Hytrel® 4056 TPC-ET

PDSX5173 / 197813

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.