MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Copper Alloy, UNS C69410, O60 Temper, Rod
Categories: Metal; Nonferrous Metal; Copper Alloy

Material Notes: Temper: Soft Anneal

Fabrication Properties: Excellent Suitability – Soldering, Brazing, Capacity for Being Hot Formed; Good Suitability – Oxyacetylene Welding, Gas Shielded Arc Welding, Coated Metal Arc Welding, Spot Weld, Seam Weld, Butt Weld; Poor Suitability – Capacity for Being Cold Worked

Typical uses: Lead-free, dezincification resistant alloy for potable water components; Low Lead Valves and Fittings

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 8.19 g/cc0.296 lb/in³
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell B  85
@Thickness 50.8 mm
85
@Thickness 2.00 in
 85
@Thickness 25.4 mm
85
@Thickness 1.00 in
 85
@Thickness 12.7 mm
85
@Thickness 0.500 in
Tensile Strength  552 MPa
@Thickness 50.8 mm
80000 psi
@Thickness 2.00 in
 586 MPa
@Thickness 25.4 mm
85000 psi
@Thickness 1.00 in
 621 MPa
@Thickness 12.7 mm
90000 psi
@Thickness 0.500 in
Tensile Strength, Yield  276 MPa
@Thickness 50.8 mm
40000 psi
@Thickness 2.00 in
0.5% Ext
 296 MPa
@Thickness 25.4 mm
43000 psi
@Thickness 1.00 in
0.5% Ext
 310 MPa
@Thickness 12.7 mm
45000 psi
@Thickness 0.500 in
0.5% Ext
Elongation at Break  20 %
@Thickness 12.7 mm
20 %
@Thickness 0.500 in
 25 %
@Thickness 50.8 mm
25 %
@Thickness 2.00 in
 25 %
@Thickness 25.4 mm
25 %
@Thickness 1.00 in
Tensile Modulus 110 GPa16000 ksi
Machinability 30 %30 %
Forgeability 80 %80 %
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 0.0000280 ohm-cm0.0000280 ohm-cm6.2% IACS
 
Thermal PropertiesMetricEnglishComments
CTE, linear 20.2 µm/m-°C
@Temperature 20.0 - 300 °C
11.2 µin/in-°F
@Temperature 68.0 - 572 °F
Thermal Conductivity 2.16 W/m-K15.0 BTU-in/hr-ft²-°F
Melting Point 821 - 918.3 °C1510 - 1685 °F
Solidus 821 °C1510 °F
Liquidus 918.3 °C1685 °F
 
Component Elements PropertiesMetricEnglishComments
Copper, Cu >= 81 %>= 81 %
Iron, Fe <= 0.20 %<= 0.20 %
Lead, Pb <= 0.090 %<= 0.090 %
Silicon, Si 3.5 - 4.5 %3.5 - 4.5 %
Zinc, Zn 11 - 15 %11 - 15 %

References for this datasheet.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

MC69410x2 / 292383

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.