MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

LyondellBasell Alathon® L5005 High Density Polyethylene
Categories: Polymer; Film; Thermoplastic; Polyethylene (PE); High Density (HDPE); High Density Polyethylene (HDPE), Film Grade

Material Notes:

Applications
ALATHON L 5005 is a high molecular weight high density copolymer that provides broad bimodal molecular weight distribution, high stiffness and good heat seal response and strength. Typical applications include merchandise bags, grocery sacks, trash can liners, produce bags and roll stock.

Regulatory Status
L 5005 meets the requirements of Food and Drug Administration regulation, 21 CFR 177.1520. This regulation allows the use of this olefin polymer in "…articles or components of articles intended for use in contact with food." Specific limitations or conditions of use may apply.

Processing Techniques
Specific recommendations for processing L 5005 can only be made when the processing conditions, equipment and end use are known.

Typical Process Condition Ranges: BUR=3.5-4.5:1; Neck Height=6-9 Die Diameters: Die Gap(nominal), in.=0.040-0.050; Tower Height=Relatively Short; Output, Lb/Hr/In of Die Circumference=10-12; Melt Temperature- 390-420°F(199-216°C)

This product is from the former Equistar product line.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.949 g/cc0.0343 lb/in³ASTM D1505
Melt Flow 0.057 g/10 min0.057 g/10 minASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Film Tensile Strength at Yield, MD 26.2 MPa3800 psiASTM D882
Film Tensile Strength at Yield, TD 23.4 MPa3400 psiASTM D882
Film Elongation at Break, MD 300 %300 %ASTM D882
Film Elongation at Break, TD 420 %420 %ASTM D882
Elmendorf Tear Strength MD 14 g14 gASTM D1922
Elmendorf Tear Strength TD 35 g35 gASTM D1922
Dart Drop Total Energy 1090 J/cm2.05 ft-lb/milASTM D3420
Film Tensile Strength at Break, MD 58.6 MPa8500 psiASTM D882
Film Tensile Strength at Break, TD 34.5 MPa5000 psiASTM D882
1% Secant Modulus, MD 793 MPa115000 psiASTM D822
1% Secant Modulus, TD 965 MPa140000 psiASTM D822
 
Processing PropertiesMetricEnglishComments
Melt Temperature 199 - 216 °C390 - 421 °F
 
Compliance PropertiesMetricEnglishComments
FDA YesYesSee notes for details.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Dow LDPE 133A Low Density Polyethylene, Blown Film Grade
LyondellBasell Alathon® L5005V High Density Polyethylene, HMW Film Grade
Borealis FS1560 High Density Polyethylene
Chevron Phillips Marlex® 1412 Injection Molding Resin
ExxonMobil Exceed™ 1018KA Metallocene Polyethylene Resin (Asia Pacific Grade)

PEQU0135 / 36564

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.