MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Superior Die Set FORTAL® HR Aluminum Alloy
Categories: Metal; Nonferrous Metal; Aluminum Alloy

Material Notes: Description: FORTAL is a high strength, lightweight, easy to machine alloy, originally developed to be used in the aerospace industry. It can be found whenever a structure is highly solicited and doesn't require a very high ratio of resistance/mass. FORTAL offers machinability, high resistance to corrosion, and leads to increased productivity. FORTAL's modulus of elasticity is one third that of steel, and can absorb three times as much shock and vibration in its elastic phase. FORTAL is solution heat-treated, stabilized, artificially aged and stress relieved by stretching.

Application: FORTAL is an ideal material for all types of products and tooling since it is stronger than 1020 steels.

Information provided by Superior Die Set.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.100 lb/in³
Thickness 14000 - 92000 micronsintermediate sizes also available
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 145
 150
Tensile Strength, Ultimate 78320 psi
Tensile Strength, Yield 69600 psi
Elongation at Break 10 %
Modulus of Elasticity 10440 ksi
Fatigue Strength 80.0 MPa
@# of Cycles 1.00e+8
test bar (22mm diam.) notched (Kt = 3)
 160 MPa
@# of Cycles 1.00e+8
test bar (22mm diam.) unnotched (Kt =1)
Shear Strength 48000 psi
 
Thermal PropertiesOriginal ValueComments
CTE, linear 13.05 µin/in-°F
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.229 BTU/lb-°F
Thermal Conductivity 130 W/m-K
Maximum Service Temperature, Air 140 °FRecommended
 
Component Elements PropertiesOriginal ValueComments
Aluminum, Al 90.07 %
Chromium, Cr 0.23 %
Copper, Cu 1.6 %
Magnesium, Mg 2.5 %
Zinc, Zn 5.6 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Superior Die Set FORTAL® HP Aluminum Alloy
Constellium Fortal® Aluminum Alloy
Aluminum 7075-T6; 7075-T651
RSP Technology RSA-501 AE Aluminum Scandium Super Alloy (Scalmalloy)
Overview of materials for Aluminum Alloy

NSUP01 / 19247

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.