MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Mitsubishi Novarex® 7025R Polycarbonate
Categories: Polymer; Thermoplastic; Polycarbonate (PC); Polycarbonate, Molded

Material Notes: Medium viscosity basic 2 grade. Used in a wide range of industries, including sports equipment, medical equipment, automobiles, optics, machinery, office automation equipment, and electronics, they have a reputation for reliability with users. Superior impact strength, Superior transparency. Usability in a wide range of temperatures: -40degC to 120degC.Excellent precision molding properties and dimensional stability. Superior self-extinguishing properties. Excellent weather resistance. Excellent electrical insulation capabilities. 7025 IR (ice color)

Information provided by Mitsubishi Engineering Plastics Corporation.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.20 g/cc0.0434 lb/in³ISO 1183
Water Absorption 0.24 %
@Temperature 23.0 °C
0.24 %
@Temperature 73.4 °F
Immersion
Linear Mold Shrinkage, Flow 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
Linear Mold Shrinkage, Transverse 0.0050 - 0.0070 cm/cm
@Thickness 3.20 mm
0.0050 - 0.0070 in/in
@Thickness 0.126 in
Melt Flow 7.4 g/10 min
@Load 1.20 kg,
Temperature 300 °C
7.4 g/10 min
@Load 2.65 lb,
Temperature 572 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 61.0 MPa8850 psiISO 527-1,2
Elongation at Break 115 %115 %ISO 527-1,2
Elongation at Yield 5.6 %5.6 %ISO 527-1,2
Tensile Modulus 2.40 GPa348 ksiISO 527-1,2
Flexural Strength 93.0 MPa13500 psiISO 178
Flexural Modulus 2.30 GPa334 ksiISO 178
Charpy Impact Unnotched NBNBISO 179-1
Charpy Impact, Notched 7.60 J/cm²36.2 ft-lb/in²ISO 179-2
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 3.00e+16 ohm-cm3.00e+16 ohm-cmIEC 60093
Surface Resistance 6.00e+15 ohm6.00e+15 ohmIEC 60093
Dielectric Constant  3.1
@Frequency 100 Hz
3.1
@Frequency 100 Hz
IEC 60250
 3.1
@Frequency 1e+6 Hz
3.1
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength  17.0 kV/mm
@Thickness 3.00 mm
432 kV/in
@Thickness 0.118 in
IEC 60243-1
 24.0 kV/mm
@Thickness 2.00 mm
610 kV/in
@Thickness 0.0787 in
IEC 60243-1
Dissipation Factor  0.00060
@Frequency 100 Hz
0.00060
@Frequency 100 Hz
IEC 60250
 0.0090
@Frequency 1e+6 Hz
0.0090
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 250 - 400 V250 - 400 VUL746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 65.0 µm/m-°C36.1 µin/in-°FISO 11359-2
CTE, linear, Transverse to Flow 66.0 µm/m-°C36.7 µin/in-°FISO 11359-2
Maximum Service Temperature, Air 120 °C248 °F
Deflection Temperature at 0.46 MPa (66 psi) 143 °C289 °FISO 75-1,2
Deflection Temperature at 1.8 MPa (264 psi) 129 °C264 °FISO 75-1,2
Minimum Service Temperature, Air -40.0 °C-40.0 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Mitsubishi Novarex® 7027R Polycarbonate
Mitsubishi Novarex® 7022R Polycarbonate
Mitsubishi Novarex® 7030R Polycarbonate
Mitsubishi Iupilon® E-2000 Polycarbonate

PMITSU9033 / 191706

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.