MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

Celanese Hytrel® DYM250S BK472 TPC-ET+PBT
Categories: Polymer; Thermoplastic; Elastomer, TPE; Polyester TPE

Material Notes: Medium Modulus Polyester Elastomer with Excellent Impact Resistance Developed for Air Bag Door Applications

Former DuPont product acquired by Celanese in 2022.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.16 g/cc0.0419 lb/in³ISO 1183
Melt Density 0.995 g/cc
@Temperature 245 °C
0.0359 lb/in³
@Temperature 473 °F
Linear Mold Shrinkage, Flow 0.012 cm/cm0.012 in/inISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.012 cm/cm0.012 in/inISO 294-4, 2577
Melt Flow  13 g/10 min
@Load 2.16 kg,
Temperature 240 °C
13 g/10 min
@Load 4.76 lb,
Temperature 464 °F
cm³/10min Volumetric; ISO 1133
 13 g/10 min
@Load 2.16 kg,
Temperature 240 °C
13 g/10 min
@Load 4.76 lb,
Temperature 464 °F
ISO 1133
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 444415s; ISO 48-4
 <= 49<= 49ISO 48-4
Tensile Stress at Strain  7.80 MPa
@Strain 5.0 %
1130 psi
@Strain 5.0 %
1BA specimen at 50mm/min; ISO 527-1/-2
 9.70 MPa
@Strain 10 %
1410 psi
@Strain 10 %
ISO 527-1/-2
 12.5 MPa
@Strain 50 %
1810 psi
@Strain 50 %
ISO 527-1/-2
 14.0 MPa
@Strain 100 %
2030 psi
@Strain 100 %
ISO 527-1/-2
 18.0 MPa
@Strain 300 %
2610 psi
@Strain 300 %
ISO 527-1/-2
Flexural Modulus 0.350 GPa50.8 ksiISO 178
Tear Strength 90.0 kN/m514 plinormal; ISO 34-1
 110 kN/m628 pliparallel; ISO 34-1
 
Thermal PropertiesMetricEnglishComments
Melting Point 222 °C432 °F10°C/min; ISO 11357-1/-3
Deflection Temperature at 0.46 MPa (66 psi) 48.0 °C118 °FISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 41.0 °C106 °FISO 75-1/-2
Brittleness Temperature -100 °C-148 °FISO 974
Flame Spread 24.0 mm/min
@Thickness 1.00 mm
0.945 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 245 °C473 °FOptimum, Injection
 240 - 250 °C464 - 482 °FRange, Injection
Mold Temperature 45.0 °C113 °FOptimum, Injection
 40.0 - 55.0 °C104 - 131 °FInjection
Drying Temperature 100 °C212 °FInjection
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection, Dehumidified Dryer
Moisture Content <= 0.050 %<= 0.050 %Injection
 
Descriptive Properties
Drying RecommendedyesInjection
Emission of organic compounds (µgC/g)9.5VDA 277
FMVSS ClassBISO 3795 (FMVSS 302)
Fogging (%)100F-value (refraction); ISO 6452
Fogging (mg)0G-value (condensate); ISO 6452
Odor Class4VDA 270
Part Marking Code>TPC-ET+PBT<ISO 11469
Polymer(TPC+PBT)
Resin IdentificationTPC-ET+PBTISO 1043

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Hytrel® DYM350BK TPC-ET+PBT
Celanese Hytrel® HTR8068 TPC-ET-FR(17)
Celanese Hytrel® HTR8223 BK320 TPC-ET
Celanese Hytrel® HTR8341C BK320 TPC-ET
DuPont Mobility and Materials Hytrel® HTR8136BK TPC-ET

PDSX5194 / 197834

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.