MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Haysite Heatmeiser® H340 Platen Insulation
Categories: Polymer; Thermoset; Polyester, TS; Thermoset Polyester Glass Filled BMC

Material Notes: Haysite’s family of mold and platen insulation products are specially engineered fiberglass reinforced thermoset polyester composites which offer superior energy efficiency, temperature control, and durability for high temperature mold and platen thermal applications. Haysite Thermalate® composites offer a number of specific advantages over other insulation materials:
  • Asbestos Free
  • Cost Effective: Increased efficiency allows for short payback
  • Low Thermal Conductivity/Energy Efficient: Saves and allows more precise temperature control
  • High Heat Resistance: Designed to operate at temperatures up to 550ºF
  • High Compressive Strength: Will not take a compressive “set”, causing mold alignment problems, when subject to extremely high molding pressures
  • Tough and Durable: Does not crack or break easily during mold setup or tear down. More durable than mica or asbestos materials
  • Resists Oils and Fluids: Other more absorbent insulators, such as concrete asbestos, can deteriorate or alter their thermal conductivity
  • No Maintenance
Information provided by Red Seal Electric Company.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Moisture Absorption at Equilibrium 0.25 %0.25 %3/8", Sanded; ASTM D570
 
Mechanical PropertiesMetricEnglishComments
Flexural Strength 141 MPa20500 psiASTM D790
Compressive Strength 125 MPa18100 psiASTM D695, Cond. A
 131 MPa
@Temperature 149 °C
19000 psi
@Temperature 300 °F
 133 MPa
@Temperature 204 °C
19300 psi
@Temperature 400 °F
 138 MPa
@Temperature 260 °C
20000 psi
@Temperature 500 °F
Izod Impact, Notched 4.81 J/cm9.00 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
CTE, linear 11.7 µm/m-°C6.50 µin/in-°FASTM D696
Thermal Conductivity 0.173 W/m-K1.20 BTU-in/hr-ft²-°FASTM D177
Maximum Service Temperature, Air 288 °C550 °F
 
Descriptive Properties
ColorLight Gray

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Gneiss
Carpenter Pyrowear® 675 Stainless Steel, Tempered 510°C, Transverse Properties

PHAY40 / 84300

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.