MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
BASF Ultramid® KR 4365 G5 BK 00100 35% Glass Filled PA6/6T FR (Dry)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 40% Glass Fiber Filled

Material Notes: Description: Partially aromatic polyamide; flame retardant based on red phosphorus; low water absorption, high melting point (295°C); low tendency to form deposits on electrical contacts, very resistant to electrolytic corrosion, resistant to soldering temperatures, can be electroplated.

Information provided by BASF

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.500 - 0.800 g/cc
Density 1.38 g/ccISO 1183
Moisture Absorption at Equilibrium 1.1 - 1.5 %23°C; 50% RH; ISO 62
Water Absorption at Saturation 5.0 - 6.0 %ISO 62
Viscosity Measurement 130ISO 307
Linear Mold Shrinkage 0.0040 cm/cmrestricted
Linear Mold Shrinkage, Flow 0.0041 cm/cmTM=320°C, TW=100°C
 0.0050 cm/cmISO 2577
Linear Mold Shrinkage, Transverse 0.010 cm/cmISO 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 150 MPa50 mm/min; ISO 527-1/-2
Elongation at Yield 3.0 %50 mm/min; ISO 527-1/-2
Modulus of Elasticity 8.30 GPaISO 527-1/-2
Izod Impact, Notched (ISO) 13.0 kJ/m²
@Temperature 23.0 °C
ISO 180/A
Charpy Impact Unnotched 75.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 13.0 kJ/m²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+13 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 4.0
@Frequency 1e+6 Hz
IEC 60250
Dissipation Factor 0.020
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 600 VTest solution A; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 - 60.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
DIN 11359-1/-2
CTE, linear, Transverse to Flow 25.0 µm/m-°C
@Temperature 23.0 - 80.0 °C
DIN 11359-1/-2
Thermal Conductivity 0.310 W/m-KDIN 52612
Melting Point 295 °CDIN 53765
Maximum Service Temperature, Air 125 °Cfor 50% loss of tensile strength after 20000hr
 150 °Cfor 50% loss of tensile strength after 5000hr
 270 °C
Deflection Temperature at 1.8 MPa (264 psi) 270 °CISO 75-1/-2
Decomposition Temperature >= 350 °C
Flammability, UL94 V-2
@Thickness >=0.370 mm
 V-0
@Thickness >=0.750 mm
 5VB
@Thickness >=1.50 mm
Ignition Temperature >= 470 °CASTM D1929
 
Processing PropertiesOriginal ValueComments
Processing Temperature 80.0 °CHopper Throat
Zone 1 300 °CFeed Zone
Zone 2 310 °CCompression
Zone 3 320 °CMetering-zone
Zone 4 320 °CNozzle
Melt Temperature >= 320 °COptimal
 310 - 330 °CInjection-molding/Extrusion
Mold Temperature 80.0 - 120 °CInjection-molding
 100 °COptimal
Drying Temperature 110 °C
Dry Time 8 hour
 
Descriptive Properties
ColorBK 00100
Commercial StatusEurope
Peripheral Screw Speed< 0.3 m/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® KR 4355 G10 BK 23215 50% Glass Filled PA6/6T (Dry)
BASF Ultramid® KR 4365 G5 35% Glass Filled PA6/6T FR (Dry)
BASF Ultramid® KR 4355 G7 BK 00564 35% Glass Filled PA6/6T (Dry)
Celanese VECTRA E115i LCP, 15% Glass Reinforced
Domo TechnylStar™ AFX 218 V50 PA6, 50% glass filled

PBASG0334 / 131967

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.