MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Asahi Kasei Leona™ FR200 Polyamide 66, Flame Retardant
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Unreinforced, Flame Retardant

Material Notes: Applications: Connectors, switches, and other electrical and electronic parts

Information provided by Asahi Kasei Corp.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.16 g/cc
Density 1.16 g/ccDry as Molded; ISO 1183
Moisture Absorption at Equilibrium 2.4 %
@Temperature 23.0 °C
50% RH; ISO 62
 2.4 %
@Temperature 23.0 °C
50% RH
Linear Mold Shrinkage, Flow 0.013 - 0.020 cm/cmAsahi Kasei
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell M 80Dry as Molded; ISO 2039
Hardness, Rockwell R 90Conditioned at 50% RH; ISO 2039
 118Dry as Molded; ISO 2039
Tensile Strength at Break 69.0 MPaConditioned at 50% RH; ISO 527
Tensile Strength 47.0 MPaConditioned at 50% RH; ASTM D638
 79.0 MPaDry as Molded; ASTM D638
Tensile Strength, Yield 44.0 MPaConditioned at 50% RH
 75.0 MPaDry as Molded
Elongation at Break 10 %Dry as Molded; ISO 527
 >= 100 %Conditioned at 50% RH; ISO 527
Elongation at Yield 3.5 %
@Temperature 23.0 °C
Dry as Molded; ISO 527
 24 %
@Temperature 23.0 °C
Conditioned at 50% RH; ISO 527
Tensile Modulus 1100 MPaConditioned at 50% RH; ISO 527
 3500 MPaDry as Molded; ISO 527
Flexural Strength 37.2 MPaConditioned at 50% RH; ISO 178
 117 MPaDry as Molded; ISO 178
Flexural Modulus 1000 MPaConditioned at 50% RH; ISO 178
 2900 MPaDry as Molded; ISO 178
Izod Impact, Notched 29.0 J/mDry as Molded; ASTM D256
 118 J/mConditioned at 50% RH; ASTM D256
Charpy Impact Unnotched NBConditioned at 50% RH; ISO 179
 NBDry as Molded; ISO 179
Charpy Impact, Notched 4.00 kJ/m²Dry as Molded; ISO 179
 11.0 kJ/m²Conditioned at 50% RH; ISO 179
Taber Abrasion, mg/1000 Cycles 8.0Conditioned at 50% RH; ASTM D1044
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+14 ohm-cmDry as Molded; IEC 60093
Surface Resistance 1.00e+13 ohmDry as Molded; IEC 60093
Dielectric Strength 19.0 kV/mmDry as Molded; IEC 60243
Comparative Tracking Index 600 V
@Thickness 3.00 mm
Dry as Molded; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 80.0 µm/m-°CDry as Molded; ASTMD 696
Deflection Temperature at 0.46 MPa (66 psi) 203 °CDry as Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 62.0 °CDry as Molded; ISO 75
Flammability, UL94 V-0
@Thickness 0.750 mm
Dry as Molded
Oxygen Index 32 %Dry as Molded; ASTM D2863
Glow Wire Flammability Index 960 °CDry as Molded; IEC 60695-2-12

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Chi Mei Kibisan® PN-117C SAN
Chi Mei Polylac® PA-757 ABS
Lotte Chemical Titan TITANPRO® 6331 Polypropylene homopolymer
Polyplastics Duracon® M90-44/M90S Acetal Co-polymer (POM), Standard, General
Celanese Zytel® 70G33HS1L BK031 PA66-GF33

PASAHI8160 / 221187

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.