MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Metal adhesives

Henkel Loctite® ABLESTIK 8200C Adhesive
Categories: Polymer; Adhesive

Material Notes: Appearance: Silver

Product Benefits:

  • High electrical conductivity
  • Improved MRT on Ag plated LF
  • Low bleed
  • Snap curable
Cure: Heat cure

Application: Die attach

Filler Type: Silver

Key Substrates: PPF, Copper and Silver

LOCTITE ABLESTIK 8200C electrically conductive die attach adhesive is designed for high reliability package applications with medium thermal and electrical requirements. This material offers improved JEDEC performance on QFN type packages.

Information provided by Loctite®

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Moisture Absorption 0.200 %0.200 %Saturation, after 85% RH exposure
Brookfield Viscosity 11500 cP11500 cPUncured, CP51, Speed 5 rpm
 
Mechanical PropertiesMetricEnglishComments
Tensile Modulus  0.759 GPa
@Temperature 250 °C
110 ksi
@Temperature 482 °F
Cured, DMTA
 1.172 GPa
@Temperature 150 °C
170.0 ksi
@Temperature 302 °F
Cured, DMTA
 4.621 GPa
@Temperature 25.0 °C
670.2 ksi
@Temperature 77.0 °F
Cured, DMTA
 
Electrical PropertiesMetricEnglishComments
Volume Resistivity 0.00017 ohm-cm0.00017 ohm-cm
 
Thermal PropertiesMetricEnglishComments
CTE, linear 60.0 µm/m-°C33.3 µin/in-°FCured, Below Tg
 130 µm/m-°C72.2 µin/in-°FCured, Above Tg
Thermal Conductivity 1.20 W/m-K8.33 BTU-in/hr-ft²-°FCured
Glass Transition Temp, Tg 190 °C374 °FCured, TMA
 
Processing PropertiesMetricEnglishComments
Cure Time 30.0 min0.500 hourramp to 175°C + 15 minutes @ 175°C
Working Life 1440 min1440 min
Shelf Life 12.0 Month
@Temperature -40.0 °C
12.0 Month
@Temperature -40.0 °F
Uncured, from date of manufacture
 
Descriptive Properties
Extractable Ionic Content (ppm)<10Cured, Chloride (Cl-)
 <10Cured, Sodium (Na+)
 <10Cured, Potassium (K+)
Shear Strength19.1 kg-fDie, x 3 mm Si die on SPCLF
Thixotropic Index5Uncured, 0.5/5 rpm
Weight Loss (%)1Cure, 300ºC

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PLOCT5026 / 255237

Metal adhesives

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.