MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Constellium Alumold® 500 Forged Aluminum
Categories: Metal; Nonferrous Metal; Aluminum Alloy; 5000 Series Aluminum Alloy

Material Notes: Forged thick blocks in Alumold® 500 have been developed to provide high and consistent strength across the thickness, good dimensional stability and excellent machinability, in order to respond to the high requirements of the applications in plastics transformation. Typical applications include compression or injection moulds for plastics.

Information provided by manufacturer

Key Words: IS 5505
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 2.82 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Brinell 150
@Thickness 450 - 700 mm
long-transverse direction
 160
@Thickness 400 - 450 mm
long-transverse direction
 165
@Thickness 300 - 400 mm
long-transverse direction
Tensile Strength >= 410 MPa
@Thickness 450 - 700 mm
long-transverse direction
 >= 430 MPa
@Thickness 400 - 450 mm
long-transverse direction
 >= 450 MPa
@Thickness 300 - 400 mm
long-transverse direction
 450 MPa
@Thickness 400 - 450 mm
long-transverse direction
 480 MPa
@Thickness 450 - 700 mm
long-transverse direction
 520 MPa
@Thickness 300 - 400 mm
long-transverse direction
Tensile Strength, Yield >= 340 MPa
@Strain 0.2 %,
Thickness 450 - 700 mm
long-transverse direction
 >= 350 MPa
@Strain 0.2 %,
Thickness 400 - 450 mm
long-transverse direction
 >= 370 MPa
@Strain 0.2 %,
Thickness 300 - 400 mm
long-transverse direction
 420 MPa
@Strain 0.2 %,
Thickness 450 - 700 mm
long-transverse direction
 460 MPa
@Strain 0.2 %,
Thickness 300 - 400 mm
long-transverse direction
 460 MPa
@Strain 0.2 %,
Thickness 400 - 450 mm
long-transverse direction
Elongation at Break >= 3.0 %
@Thickness 300 - 400 mm
long-transverse direction
 >= 3.0 %
@Thickness 400 - 450 mm
long-transverse direction
 >= 3.0 %
@Thickness 450 - 700 mm
long-transverse direction
 7.0 %
@Thickness 400 - 450 mm
long-transverse direction
 7.0 %
@Thickness 450 - 700 mm
long-transverse direction
 8.0 %
@Thickness 300 - 400 mm
long-transverse direction
Modulus of Elasticity 73.0 GPacompression
Tensile Modulus 72.0 GPa
Poissons Ratio 0.33
 
Thermal PropertiesOriginal ValueComments
CTE, linear 23.7 µm/m-°C
@Temperature 20.0 - 100 °C
Specific Heat Capacity 0.857 J/g-°C
Thermal Conductivity 153 W/m-K
 
Descriptive Properties
Thermal Diffusivity63 mm²/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Constellium Alumold® 500 Rolled Aluminum
PCP-Canada Max 5® 5083 Cast Aluminum Mold Block
Clinton Aluminum Alumold® 1-500 Forged
ALIMEX PLANAL 7075 T651/T652 Aluminum Alloy
ALIMEX AMP 8000 Aluminum Plate

NCONS015 / 160278

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.