MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Ensinger PEI

(Viewing data as-entered. Click here to return)
Pressure Seal 9901 Fluorinated Hydrocarbon
Categories: Polymer; Thermoset; Rubber or Thermoset Elastomer (TSE)

Material Notes: Compound 9901 is a 90 durometer black colored Fluorinated Hydrocarbon elastomer. It is specifically formulated for low temperature applications, it has a true TR-10 of -40°C(-40°F). It also exhibits good resistance to compression set, petroleum based oils, aliphatic and aromatic fuels and oxygenated fuels.

This compound will meet or exceed the specifications listed and has the following physical properties: ASTM D2000 3 HK 920 A1-10 B37 B38 EO78; 5 HK 920 A1-11 B38 EO78 F15; 7 HK 920 A1-10 A1-11 B38 EO88 F15

Information provided by Pressure Seals Inc.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.86 g/cc
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 88
 78
@Temperature 200 °C,
Time 252000 sec
Stauffer Blend 7700
 85
@Temperature 200 °C,
Time 252000 sec
Service Fluid 101
 85
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 86
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 87
@Temperature 275 °C,
Time 252000 sec
Heat Aged
 87
@Temperature 100 °C,
Time 252000 sec
Distilled water aged
 88
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 88
@Temperature 250 °C,
Time 252000 sec
Heat Aged
Tensile Strength 2257 psi
 1503.1 psi
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 1746.9 psi
@Temperature 275 °C,
Time 252000 sec
Heat Aged
 1972.6 psi
@Temperature 250 °C,
Time 252000 sec
Heat Aged
 1999.7 psi
@Temperature 200 °C,
Time 252000 sec
Stauffer Blend 7700
 2013.2 psi
@Temperature 200 °C,
Time 252000 sec
Service Fluid 101
 2277.3 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
 2484.9 psi
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
Elongation, Ultimate 123 %
 29.4 %
@Temperature 275 °C,
Time 252000 sec
Heat Aged
 99.3 %
@Temperature 23.0 °C,
Time 252000 sec
ASTM Reference Fuel C
 109.8 %
@Temperature 250 °C,
Time 252000 sec
Heat Aged
 124.1 %
@Temperature 200 °C,
Time 252000 sec
Stauffer Blend 7700
 125.2 %
@Temperature 200 °C,
Time 252000 sec
Service Fluid 101
 129.8 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #1 (IRM 901)
 133.2 %
@Temperature 150 °C,
Time 252000 sec
ASTM Oil #3 (IRM 903)
50% Modulus 902 psi
100% Modulus 1853 psi
Tear Strength 98.0 pliDie B
 129 pliDie C
Compression Set 7.8 %
@Temperature 175 °C,
Time 79200 sec
Plied
 9.3 %
@Temperature 200 °C,
Time 79200 sec
Plied
 16.2 %
@Temperature 23.0 °C,
Time 79200 sec
Plied
 
Thermal PropertiesOriginal ValueComments
Brittleness Temperature -19.0 °F
Shrinkage 1.0 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #3
 1.8 %
@Temperature 150 °C,
Time 252000 sec
Volume, ASTM Oil #1
 2.9 %
@Temperature 100 °C,
Time 252000 sec
Volume, Distilled water aged
 5.0 %
@Temperature 23.0 °C,
Time 252000 sec
Volume, ASTM Reference Fuel C
 6.6 %
@Temperature 200 °C,
Time 252000 sec
Volume, Service Fluid 100
 12.9 %
@Temperature 200 °C,
Time 252000 sec
Volume, Stauffer Blend 7700
 
Descriptive Properties
ColorBlack
TR-10 Temperature-41°C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PPRESL131 / 318341

Visit Zeus Inc. for PEEK Tubing

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.