MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 3180 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 3100 series are engineered materials designed primarily general purpose, automotive and industrial applications requiring a good balance of thermal, mechanical, and physical properties. Sarlink 3180, available in NAT and BLK, is a medium hardness, low density, multi-purpose thermoplastic vulcanizate that can be processed by injection molding, blow molding or extrusion for applications such as grips, seals, gaskets, profiles, hose & tubes, bellows, and other articles.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; General Purpose; Good Adhesion; Good Flexibility; Good Moldability; Good Processability; Good Surface Finish; Heat Aging Resistant; Medium Hardness; Resilient; Weather Resistant

Uses: Agricultural Applications; Appliance Components; Automotive Applications; Automotive Exterior Parts; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; General Purpose; Industrial Applications; Profiles; Rubber Replacement; Seals; Tubing

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-80 Type D Color: Black; CHRYSLER MS-AR-80 Type D Color: Natural; DAIMLER DBL 5556.21 Color: Black; DAIMLER DBL 5562.30 Color: Black; Food WSD-M2D381-A1 Color: Black; GM QK 3523 Type 5 Color: Natural; GM QK 3523 Type 5 Color: Black; SAE J3000 Color: Black; SAE J3000 Color: Natural; VAG VW501 79 Color: Black; VAG VW-TL 526 22 Color: Black; VOLSKWAGEN VW 50180 Color: Black

UL File Number: QMFZ2.E54709

Agency Ratings: UL 94

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.950 g/cc0.0343 lb/in³ASTM D792
Viscosity 290 cP
@Shear Rate 206 1/s,
Temperature 200 °C
290 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  80
@Time 5.00 sec
80
@Time 0.00139 hour
Extruded; ISO 868
 84
@Time 5.00 sec
84
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength at Break 8.48 MPa1230 psiFlow; ISO 37
 9.38 MPa1360 psiAcross Flow; ISO 37
 8.53 MPa
@Treatment Temp. 135 °C,
Time 360000 sec
1240 psi
@Treatment Temp. 275 °F,
Time 100 hour
Across Flow, Change in Air; ISO 188
 8.63 MPa
@Treatment Temp. 150 °C,
Time 605000 sec
1250 psi
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
Tensile Stress at Strain  4.50 MPa
@Strain 100 %
653 psi
@Strain 100 %
Across Flow; ISO 37
 6.70 MPa
@Strain 100 %
972 psi
@Strain 100 %
Flow; ISO 37
 4.91 MPa
@Strain 100 %,
Treatment Temp. 150 °C
712 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air, 168 hr; ISO 188
 5.27 MPa
@Strain 100 %,
Treatment Temp. 135 °C
764 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air, 1000 hr; ISO 188
Elongation at Break 330 %330 %Flow; ISO 37
 690 %690 %Across Flow; ISO 37
Tear Strength 50.8 kN/m290 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  32 %
@Temperature 22.8 °C,
Time 79200 sec
32 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 50 %
@Temperature 70.0 °C,
Time 79200 sec
50 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 65 %
@Temperature 90.0 °C,
Time 252000 sec
65 %
@Temperature 194 °F,
Time 70.0 hour
ISO 815
 
Thermal PropertiesMetricEnglishComments
Flammability, UL94 HB
@Thickness 1.52 mm
HB
@Thickness 0.0600 in
All Colors
 
Processing PropertiesMetricEnglishComments
Processing Temperature 185 - 220 °C365 - 428 °FInjection, Melt
Rear Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Middle Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Front Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Nozzle Temperature 187 - 220 °C369 - 428 °FInjection
Zone 1 180 - 200 °C356 - 392 °FExtrusion
Zone 2 180 - 205 °C356 - 401 °FExtrusion
Zone 3 187 - 210 °C369 - 410 °FExtrusion
Zone 4 187 - 210 °C369 - 410 °FExtrusion
Die Temperature 195 - 215 °C383 - 419 °FExtrusion
Melt Temperature 195 - 215 °C383 - 419 °FExtrusion
Mold Temperature 10.0 - 55.0 °C50.0 - 131 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Back Pressure 0.100 - 1.00 MPa14.5 - 145 psiInjection
Screw Speed 100 - 200 rpm100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1144 / 237635

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.