MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Teknor Apex Sarlink® TPE ME-2385B BLK Thermoplastic Elastomer
Categories: Polymer; Thermoplastic; Elastomer, TPE

Material Notes: Notes: Sarlink ME-2385B BLK is a high performance injection molding thermoplastic elastomer designed for automotive applications, including exterior parts exhibiting sunlight resistance and UV absorbing characteristics.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Filled; High Gloss; Light Stabilized; Low Density; Low Specific Gravity; Lubricated; Medium Flow; Slip; Sunlight Resistant; UV Absorbing

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Exterior Trim

RoHS Compliance: RoHS Compliant

Form: Pellets

Processing Method: Injection Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 0.910 g/ccISO 1183
Viscosity 192 cP
@Shear Rate 206 1/s,
Temperature 200 °C
ASTM D3835
Melt Flow 10 g/10 min
@Load 2.16 kg,
Temperature 230 °C
ASTM D1238
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore A 81
@Time 15.0 sec
Injection Molded; ISO 868
 84
@Time 5.00 sec
Injection Molded; ISO 868
 86
@Time 1.00 sec
Injection Molded; ISO 868
 83.5
@Treatment Temp. 125 °C,
Time 15.0 sec
Change in Air, 168 hr; ISO 888
 83.7
@Treatment Temp. 110 °C,
Time 15.0 sec
Change in Air, 1008 hr; ISO 888
 87.1
@Treatment Temp. 125 °C,
Time 5.00 sec
Change in Air, 168 hr; ISO 888
 87.8
@Treatment Temp. 110 °C,
Time 5.00 sec
Change in Air, 1008 hr; ISO 888
 89.4
@Treatment Temp. 125 °C,
Time 1.00 sec
Change in Air, 168 hr; ISO 888
 89.6
@Treatment Temp. 110 °C,
Time 1.00 sec
Change in Air, 1008 hr; ISO 888
Tensile Strength at Break 1320 psiFlow, Type 1, 20 in/min; ISO 37
 2000 psiAcross Flow, Type 1, 20 in/min; ISO 37
 1080 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 1140 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 1910 psi
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
 1940 psi
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
Tensile Stress at Strain 525 psi
@Strain 100 %
Across Flow, Type 1, 20 in/min; ISO 37
 637 psi
@Strain 100 %
Flow, Type 1, 20 in/min; ISO 37
 561 psi
@Strain 100 %,
Treatment Temp. 125 °C
Across Flow, Type 1, Change in Air, 168 hr; ISO 188
 566 psi
@Strain 100 %,
Treatment Temp. 110 °C
Across Flow, Type 1, Change in Air, 1008 hr; ISO 188
 713 psi
@Strain 100 %,
Treatment Temp. 110 °C
Flow, Type 1, Change in Air, 1008 hr; ISO 188
 720 psi
@Strain 100 %,
Treatment Temp. 125 °C
Flow, Type 1, Change in Air, 168 hr; ISO 188
Elongation at Break 620 %Flow, Type 1, 20 in/min; ISO 37
 830 %Across Flow, Type 1, 20 in/min; ISO 37
 496 %
@Treatment Temp. 125 °C,
Time 605000 sec
Flow, Type 1, Change in Air; ISO 188
 521 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Flow, Type 1, Change in Air; ISO 188
 791 %
@Treatment Temp. 125 °C,
Time 605000 sec
Across Flow, Type 1, Change in Air; ISO 188
 800 %
@Treatment Temp. 110 °C,
Time 3.629e+6 sec
Across Flow, Type 1, Change in Air; ISO 188
Tear Strength 240 pliAcross Flow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
 260 pliFlow, Method Ba, Angle (Unnicked), 20 in/min; ISO 34-1
Compression Set 20 %
@Temperature 22.8 °C,
Time 79200 sec
Type 1; ISO 815
 32 %
@Temperature 70.0 °C,
Time 79200 sec
Type 1; ISO 815
 37 %
@Temperature 90.0 °C,
Time 252000 sec
Type 1; ISO 815
 49 %
@Temperature 125 °C,
Time 252000 sec
Type 1; ISO 815
 
Processing PropertiesOriginal ValueComments
Rear Barrel Temperature 390 - 410 °F
Middle Barrel Temperature 400 - 420 °F
Front Barrel Temperature 410 - 430 °F
Nozzle Temperature 420 - 440 °F
Melt Temperature 420 - 440 °F
Mold Temperature 95.0 - 150 °F
Injection Pressure 200 - 1000 psi
Back Pressure 25.0 - 125 psi
Cushion 0.150 - 1.00 in
Screw Speed 50 - 120 rpm
 
Descriptive Properties
AppearanceNatural Color

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PTEKNQ1076 / 237567

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.