MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
CHT Group Magnifoam™ MF1-6535™ MTI Silicones Silicone Foam
Categories: Polymer; Thermoset; Silicone; Silicone Foam

Material Notes: Part of the Amber Chemical Group. Data provided by manufacturer.

Formerly Amber Chemical Co (ACC Silicones), aquired by CHT in 2017

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 6.50 lb/ft³ASTM D1056
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 12.0 psiASTM D412
Elongation at Break 100 %ASTM D412
Compression Set 0.00 %
@Temperature 100 °C
at 50%, 22 hrs; ASTM D1056
 0.00 %
@Temperature 70.0 °C,
Time 79200 sec
at 50%; ASTM D1056
 
Thermal PropertiesOriginal ValueComments
Flammability Test <= 25ASTM E162/D 3675
Smoke Density 1.5 min<20; ASTM E662
 4.0 min<50; ASTM E662
 
Descriptive Properties
Durability0% Height LossJounce & Squirm (1,000,000 cycles)
IFD, lbs35ASTM S3574 B1 @ 1" thick
Noise Reduction-Coefficient0.65ASTM C423-90a
Thermal Resistance, ft2-h/BTU2.7ASTM C518
Toxic Gas Emission PassBombardier SMP 800C
Vertical FlammabilityPassFAR25.83(a)(1)(i) 12sec
 PassFAR25.83(a)(1)(i) 60sec

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
DuPont Mobility and Materials Vespel® SF-0920 Polyimide Foam, Low Density
3M Techical Ceramics Ekasic® C Silicone Carbide
Calcium Carbonate (aragonite), CaCO3
Mid-Mountain Materials ARMATEX® SF7 Silicone Rubber Coated Glass Fabric
Overview of materials for Silicone Foam

PACC075 / 22202

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.