MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Sumitomo Bakelite KINEL® SK4525 S5A BMI Molding Compound
Categories: Polymer; Thermoset

Material Notes: KINEL® SK4525 S5A is a long glass fiber reinforced BMI molding compound with excellent mechanical and thermal properties.

Information provided by Sumitomo Bakelite High Performance Plastics (sbhpp)

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.66 g/ccISO 1183
Apparent Bulk Density 0.590 g/ccISO 60
Water Absorption 0.26 %ISO 62
Linear Mold Shrinkage 0.0015 cm/cmISO 2577
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 80.0 MPa
@Temperature 250 °C
ISO 178
 98.0 MPa
@Temperature 150 °C
ISO 178
 130 MPa
@Temperature 23.0 °C
ISO 178
Elongation at Break 0.60 %
@Temperature 23.0 °C
ISO 527-1
 0.60 %
@Temperature 150 °C
ISO 527-1
 0.70 %
@Temperature 250 °C
ISO 527-1
Tensile Modulus 14.0 GPa
@Temperature 250 °C
ISO 527-1
 18.0 GPa
@Temperature 150 °C
ISO 527-1
 28.0 GPa
@Temperature 23.0 °C
ISO 527-1
Flexural Strength 135 MPa
@Temperature 250 °C
ISO 178
 287 MPa
@Temperature 150 °C
ISO 178
 325 MPa
@Temperature 23.0 °C
ISO 178
Flexural Modulus 13.0 GPa
@Temperature 250 °C
ISO 178
 23.0 GPa
@Temperature 150 °C
ISO 178
 26.0 GPa
@Temperature 23.0 °C
ISO 178
Compressive Strength 127 MPa
@Temperature 250 °C
ISO 604
 219 MPa
@Temperature 150 °C
ISO 604
 306 MPa
@Temperature 23.0 °C
ISO 604
Charpy Impact, Notched 52.0 kJ/m²ISO 179-1
 
Electrical PropertiesOriginal ValueComments
Comparative Tracking Index 275 VIEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 11.0 µm/m-°CTMA
CTE, linear, Transverse to Flow 45.0 µm/m-°CTMA
Glass Transition Temp, Tg 275 °CTMA
Shrinkage 0.00 %Post; ISO 2577

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Vyncolit Neopreg Kinel® SK4525 S5 Glass Fiber Reinforced Molding Compound
Vyncolit Neopreg Kinel® SK4503 S5 Aramid Reinforced Molding Compound
Hexcel® HexPly® F655 Bismaleimide Resin, Carbon Fabric Form
Hexcel® HexPly® F655 Bismaleimide Resin
Hexcel® HexPly® F652 Bismaleimide Resin, Carbon Tape Form

PSUMIT169 / 193974

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.