MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Evonik Vestodur® 1000 Low Viscosity PBT  (discontinued **)
Categories: Polymer; Thermoplastic; Polyester, TP; Polybutylene Terephthalate (PBT); Polybutylene Terephthalate (PBT), Unreinforced, Molded

Material Notes: Description: Degussa AG’s High Performance Polymers Business Unit manufactures a range of polybutylene terephthalate compounds that are supplied under the registered trademark VESTODUR® . Material properties characterizing VESTODUR compounds are:
  • high thermostability
  • high stiffness
  • low water absorption resulting in high dimensional stability
  • high hardness
  • good strength
  • good sliding friction behavior, low abrasion
  • good creep behavior
  • good electrical properties
  • good chemical resistance
  • good weathering resistance
  • good processability
  • no tendency to form stress cracks

Specific Notes for this Material: Low- to- high-viscosity base types for injection molding applications (e.g., headlight housings, parts in medical technology) and extrusion applications (fiber optic jacketing)

Information provided by degussa.

Evonik Industries is the successor company to Degussa.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.31 g/ccISO 1183
Water Absorption at Saturation 0.45 %ISO 62
Linear Mold Shrinkage 0.015 cm/cmPigmentation can change mold shrinkage.
Linear Mold Shrinkage, Transverse 0.015 cm/cmPigmentation can change mold shrinkage.
Melt Flow 58.95 g/10 min
@Load 2.16 kg,
Temperature 250 °C
ISO 1133
 
Mechanical PropertiesOriginal ValueComments
Hardness, Shore D 79ISO 868
Ball Indentation Hardness 160 MPaH30; ISO 2039-1
Tensile Strength, Yield 55.0 MPa50 mm/min; ISO 527-1/2
Elongation at Break >= 50 %50 mm/min; ISO 527-1/2
Elongation at Yield 4.0 %50 mm/min; ISO 527-1/2
Tensile Modulus 2.60 GPaISO 527-1/2
Charpy Impact Unnotched 18.5 J/cm²
@Temperature -30.0 °C
ISO 179/1eU
 20.0 J/cm²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 0.450 J/cm²
@Temperature -30.0 °C
ISO 179/1eA
 0.500 J/cm²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+15 ohm-cmIEC 60093
Surface Resistance 1.00e+13 ohmIEC 60093
Dielectric Constant 3.3
@Frequency 100 Hz
IEC 60250
 3.5
@Frequency 1e+6 Hz
IEC 60250
Dielectric Strength 27.0 kV/mmK20/P50; IEC 60243-1
Dissipation Factor 0.0020
@Frequency 100 Hz
IEC 60250
 0.023
@Frequency 1e+6 Hz
IEC 60250
Comparative Tracking Index 575 VTest Solution A, 100 drops; IEC 60112
 600 VTest Solution A, CTI; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear 110 µm/m-°C
@Temperature 23.0 - 55.0 °C
Longitudinal; ISO 11359
CTE, linear, Transverse to Flow 110 µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359
Melting Point 221 - 226 °CDSC
Deflection Temperature at 0.46 MPa (66 psi) 150 °CISO 75-1/2
Deflection Temperature at 1.8 MPa (264 psi) 55.0 °CISO 75-1/2
Vicat Softening Point 180 °C50N; ISO 306
 220 °C10N; ISO 306
Flammability, UL94 HB
@Thickness 0.800 mm
 HB
@Thickness 1.60 mm
Oxygen Index 23 %ISO 4589
Glow Wire Test 850 °C
@Thickness 2.00 mm
IEC 60695-2-1/0-3
 
Descriptive Properties
Electrolytic CorrosionA1 StepIEC 60426

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Evonik Vestodur® GF 20 20% Glass Reinforced PBT
BASF Ultradur® FRee B 4450 G5 LS 25% Glass Filled PBT
BASF Ultradur® B 4520 High Speed PBT
Menzolit Menzolit® SMC 1650 Unsaturated Polyester UP
BASF Ultradur® B 4520 PBT

PHUMA00 / 47514

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.