MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
EMS-Grivory Grilon® AS/2 PA66
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66)

Material Notes: Product description: Grilon AS/2 is an unreinforced PA66 injection molding grade. Grilon AS/2 has the following important properties:
  • Good flow behavior
  • Easy processing
  • Short cycle times
Grilon AS/2 is used typically in applications such as cable ties, clamps, handles, spectacle frames, and furniture components.

Information provided by EMS Grivory.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.14 g/ccDry; ISO 1183
Water Absorption 8.0 %Sim. to ISO 62
Moisture Absorption 2.00 %Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.0080 cm/cmISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.012 cm/cmISO 294-4, 2577
 
Mechanical PropertiesOriginal ValueComments
Ball Indentation Hardness 85.0 MPaConditioned; ISO 2039-1
 150 MPaDry; ISO 2039-1
Tensile Strength at Break 80.0 MPaDry; ISO 527-1/-2
Tensile Strength, Yield 60.0 MPaConditioned; ISO 527-1/-2
 95.0 MPaDry; ISO 527-1/-2
Elongation at Break 10 %Nominal, Dry; ISO 527-1/-2
 >= 50 %Nominal, Conditioned; ISO 527-1/-2
Elongation at Yield 4.0 %Dry; ISO 527-1/-2
 12 %Conditioned; ISO 527-1/-2
Tensile Modulus 1700 MPaConditioned; ISO 527-1/-2
 3700 MPaDry; ISO 527-1/-2
Charpy Impact Unnotched NB
@Temperature 23.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature -30.0 °C
Conditioned; ISO 179/1eU
 NB
@Temperature 23.0 °C
Dry; ISO 179/1eU
 NB
@Temperature -30.0 °C
Dry; ISO 179/1eU
Charpy Impact, Notched 4.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 179/1eA
 4.00 kJ/m²
@Temperature -30.0 °C
Dry; ISO 179/1eA
 4.00 kJ/m²
@Temperature -30.0 °C
Conditioned; ISO 179/1eA
 12.0 kJ/m²
@Temperature 23.0 °C
Conditioned; ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Volume Resistivity 1.00e+10 ohm-cmConditioned; IEC 60093
 1.00e+12 ohm-cmDry; IEC 60093
Surface Resistance 1.00e+11 ohmIEC 60093
Dielectric Strength 27.0 kV/mmConditioned; IEC 60243-1
 29.0 kV/mmDry; IEC 60243-1
Comparative Tracking Index 600 VConditioned; IEC 60112
 
Thermal PropertiesOriginal ValueComments
CTE, linear, Parallel to Flow 50.0 µm/m-°CISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°CISO 11359-1/-2
Melting Point 260 °C10°C/min; ISO 11357-1/-3
Maximum Service Temperature, Air 80.0 - 100 °CLong Term; ISO 2578
 220 °CShort Term; EMS
Deflection Temperature at 0.46 MPa (66 psi) 225 °CISO 75-1/-2
Deflection Temperature at 1.8 MPa (264 psi) 75.0 °CISO 75-1/-2
Flammability, UL94 HBIEC 60695-11-10
 
Descriptive Properties
AutomotiveHydraulic systems
 Powertrain and Chassis
Electricals & ElectronicsCables & Tubes
FormGranules
Industry & Consumer goodsHousewares
 Hydraulics & Pneumatics
 Mechanical Engineering
 Sports & Leisure
 Tools & Accessories
ProcessingInjection Molding
Product AttributesNucleated

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
BASF Ultramid® B3K BK00464 PA6 (Conditioned)
EMS-Grivory Grilon® BS/2 PA6
EMS-Grivory Grilon® AS V0 PA66
BASF Ultramid® 1310-11 NF2001 PA66 (Dry)
EMS-Grivory Grilon® AS LF 20 PA66-Z20

PGRH157 / 156866

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.