MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Encom Polymers EnValoy F0PC/ABS PC/ABS Alloy, Flame Retardant, UV Stabilized Injection Grade
Categories: Polymer; Thermoplastic; ABS Polymer; Polycarbonate/ABS Alloy, Unreinforced

Material Notes: Appearance: Black, Natural or Colors

Processing Methods: Injection Molding

Applications: Appliance, Tool and Equipment, Electrical Components

Information provided by EnCom Polymers

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.18 g/cc1.18 g/ccASTM D792
Maximum Moisture Content 0.0400.040
Linear Mold Shrinkage, Flow 0.0050 cm/cm
@Thickness 3.20 mm
0.0050 in/in
@Thickness 0.126 in
ASTM D955
Melt Flow 18 g/10 min
@Load 2.16 kg,
Temperature 260 °C
18 g/10 min
@Load 4.76 lb,
Temperature 500 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 61.0 MPa8850 psiASTM D638
Elongation at Break 40 %40 %ASTM D638
Flexural Strength 93.0 MPa13500 psiASTM D790
Flexural Modulus 2.621 GPa380.1 ksiASTM D790
Izod Impact, Notched 5.34 J/cm10.0 ft-lb/inASTM D256
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 102 °C216 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 94.0 °C201 °FASTM D648
Flammability, UL94 V-0
@Thickness 1.59 mm
V-0
@Thickness 0.0625 in
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 216 - 249 °C420 - 480 °F
Middle Barrel Temperature 216 - 260 °C420 - 500 °F
Front Barrel Temperature 238 - 271 °C460 - 520 °F
Nozzle Temperature 238 - 271 °C460 - 520 °F
Melt Temperature 238 - 271 °C460 - 520 °F
Mold Temperature 54.4 - 82.2 °C130 - 180 °F
Drying Temperature 85.0 °C185 °F
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hour

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PENCOM128 / 266142

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.