MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

CRP  Windform

(Viewing data as-entered. Click here to return)
Clariant Natural Polycarbonate 3D Printer Filament
Categories: Polymer; 3D Printing/Additive Manufacturing Polymer; Thermoplastic; Polycarbonate (PC)

Material Notes: Due to its strength, impact resistance and chemical resistance, polycarbonate is a very attractive material for engineering products. Clariant polycarbonate 3D printer filament is made with a high performance, general purpose and high flow polycarbonate that provides end use parts of excellent quality. A specially formulated Renol® masterbatch is added to improve the processability during 3D printing.

General properties:

  • Amorphous thermoplastic
  • Strong and tough engineering thermoplastic
  • High impact strength
  • Highly transparent material
Available in a variety of standard colors.

Information provided by Clariant.

Vendors:
Proto3000 provides design tools, 3D printers, additive manufacturing processes, metrology technologies, high-performance materials, and part-finishing automation. Our ISO 9001:2015 additive manufacturing production facility offers 3D printing services, rapid prototyping services, and end-part production with HP MultiJet Fusion (MJF), FDM, SLA, SLS, Polyjet, DLP, metal binder jetting, BMD, and DMLS.

Click here to view all available suppliers for this material.

Please click here if you are a supplier and would like information on how to add your listing to this material.

 
Physical PropertiesOriginal ValueComments
Density 1.193 g/ccISO 1183
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Yield 64.0 MPa50 mm/min, Injection Molded; ISO 527
Elongation at Break 58 %50 mm/min, Injection Molded; ISO 527
Flexural Strength 90.0 MPaInjection Molded; ISO 178
Flexural Modulus 2.30 GPaInjection Molded; ISO 178
Izod Impact, Notched (ISO) 55.0 kJ/m²Injection Molded; ISO 180
Charpy Impact, Notched 5.60 J/cm²Injection Molded; ISO 180
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 0.46 MPa (66 psi) 138 °CInjection Molded; ISO 75
Deflection Temperature at 1.8 MPa (264 psi) 123 °CInjection Molded; ISO 75
Glass Transition Temp, Tg 142 - 145 °CDSC at 10°C/min; ISO 11357
 
Processing PropertiesOriginal ValueComments
Processing Temperature 260 - 300 °CPrint Temperature
 
Descriptive Properties
Printing Bed AdhesionPEI surfaceDirect
 PET or Polyimide tape with thin coat of PVP or EVA adhesive
Printing Bed Temperature110-130°C Ideal
Printing Fan SettingOff to Low
Printing Speed20 - 40 mm/s

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Aclo Accucomp Polycarbonate POL051L Medium Viscosity
Evonik Vestodur® 2000 Medium Viscosity PBT
Mitsubishi Xantar® 24 R Polycarbonate
Covestro Apec® HT KU 1-9331 High-Heat Polycarbonate
Cossa Polimeri ESTACARB 0501 Polycarbonate

PCLAR00005 / 230597

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.