MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

Plastics Group Polifil® 930L-33GF Glass Fiber-Reinforced Nylon 6 (DAM)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 6 (PA6); Nylon 6, 40% Glass Fiber Filled

Material Notes: Polifil® GFN/MRN 6 reinforced series of compounds provide good heat and dimensional stability and offer extended or continuous stability under high temperatures. These have been found useful in industrial clamp components as well as bearings. Standard processing techniques are applicable.

Information provided by The Plastics Group.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.36 g/cc1.36 g/ccASTM D792
Density 1.36 g/cc0.0491 lb/in³ASTM D792
Filler Content 33.0 %33.0 %TPG WI
Water Absorption 1.1 %1.1 %24 hours; ASTM D570
 1.10 %
@Time 86400 sec
1.10 %
@Time 24.0 hour
ASTM D570
Linear Mold Shrinkage  0.0030 cm/cm
@Thickness 3.17 mm
0.0030 in/in
@Thickness 0.125 in
ASTM D955
 0.00300 cm/cm
@Thickness 3.17 mm
0.00300 in/in
@Thickness 0.125 in
ASTM D955
 
Mechanical PropertiesMetricEnglishComments
Hardness, Rockwell R 119119ASTM D785
 119119ASTM D785
Tensile Strength at Break 159 MPa23000 psiASTM D638
Tensile Strength 159 MPa23000 psiASTM D638
Elongation at Break 3.0 %3.0 %ASTM D638
 3.00 %3.00 %ASTM D638
Elongation at Yield 2.0 %2.0 %ASTM D638
 2.00 %2.00 %ASTM D638
Tensile Modulus 9.31 GPa1350 ksiASTM D638
Flexural Strength 207 MPa30000 psiASTM D790
 207 MPa30000 psiASTM D790
Flexural Modulus 8.27 GPa1200 ksiTangent; ASTM D790
 8.27 GPa1200 ksitangent; ASTM D790
Izod Impact, Notched 1.07 J/cm2.00 ft-lb/inAt 73°F; ASTM D256
 1.07 J/cm2.00 ft-lb/inASTM D256
Gardner Impact 0.452 J
@Thickness 12.7 mm
0.333 ft-lb
@Thickness 0.500 in
tup; ASTM D5420
 
Thermal PropertiesMetricEnglishComments
Melting Point 216 °C420 °FASTM D789
Deflection Temperature at 0.46 MPa (66 psi) 216 °C420 °FASTM D648
 216 °C420 °FASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 210 °C410 °FASTM D648
 210 °C410 °FASTM D648
 
Processing PropertiesMetricEnglishComments
Rear Barrel Temperature 249 °C480 °F
Middle Barrel Temperature 271 °C520 °F
Front Barrel Temperature 282 °C540 °F
Nozzle Temperature 282 °C540 °F
Melt Temperature 277 - 293 °C530 - 560 °F
Mold Temperature 37.8 - 93.3 °C100 - 200 °F
Drying Temperature 104 °C
@Time 7200 sec
219 °F
@Time 2.00 hour
Back Pressure 0.172 - 0.517 MPa25.0 - 75.0 psi
Screw Speed 30.0 - 60.0 rpm30.0 - 60.0 rpm

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Global Atron Nylon 6 UIM 33 GF Nylon 6 33% Glass Filled, Impact Modified Black
Overview of materials for Polyetheretherketone, PTFE Filled
BASF Ultramid® B3EG6 30% Glass Filled PA6 (Dry)
BASF Ultramid® B3EG6 30% Glass Filled PA6 (Conditioned)
BASF Ultramid® B3EG3 15% Glass Filled PA6 (Conditioned)

PPOLI045 / 56949

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.