MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

Sandvik SANMAC 4435 Bar Steel
Categories: Metal; Ferrous Metal; Austenitic

Material Notes: Sandvik SANMAC 316L, 1.4435, with improved machinability is an austenitic chromium-nickel steel with minimum 2.5% molybdenum. Industrial Categories:
  • Chemical Industry
  • Food Industry
  • Petrochemical Industry
  • Pilp and Paper Industry
  • Nuclear Industry
  • Typical Applications:

  • Flanges
  • Valves
  • Fittings
  • Couplings
  • Rings
  • Seals
  • Bolts and Nuts
  • Shafts
  • Forgings
  • Discs
  • Information provided by Sandvik

    Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
     
    Physical PropertiesMetricEnglishComments
    Density 8.00 g/cc0.289 lb/in³
     
    Mechanical PropertiesMetricEnglishComments
    Hardness, Brinell <= 215<= 215
    Tensile Strength, Ultimate 515 - 690 MPa74700 - 100000 psi
     >= 370 MPa
    @Temperature 300 °C
    >= 53700 psi
    @Temperature 572 °F
     >= 380 MPa
    @Temperature 200 °C
    >= 55100 psi
    @Temperature 392 °F
     >= 420 MPa
    @Temperature 100 °C
    >= 60900 psi
    @Temperature 212 °F
    Tensile Strength, Yield  >= 205 MPa
    @Strain 0.2 %
    >= 29700 psi
    @Strain 0.2 %
     >= 240 MPa
    @Strain 1 %
    >= 34800 psi
    @Strain 1 %
     >= 100 MPa
    @Strain 0.2 %,
    Temperature 500 °C
    >= 14500 psi
    @Strain 0.2 %,
    Temperature 932 °F
     >= 108 MPa
    @Strain 0.2 %,
    Temperature 400 °C
    >= 15700 psi
    @Strain 0.2 %,
    Temperature 752 °F
     >= 119 MPa
    @Strain 0.2 %,
    Temperature 300 °C
    >= 17300 psi
    @Strain 0.2 %,
    Temperature 572 °F
     >= 128 MPa
    @Strain 1 %,
    Temperature 500 °C
    >= 18600 psi
    @Strain 1 %,
    Temperature 932 °F
     >= 135 MPa
    @Strain 1 %,
    Temperature 400 °C
    >= 19600 psi
    @Strain 1 %,
    Temperature 752 °F
     >= 137 MPa
    @Strain 0.2 %,
    Temperature 200 °C
    >= 19900 psi
    @Strain 0.2 %,
    Temperature 392 °F
     >= 145 MPa
    @Strain 1 %,
    Temperature 300 °C
    >= 21000 psi
    @Strain 1 %,
    Temperature 572 °F
     >= 165 MPa
    @Strain 0.2 %,
    Temperature 100 °C
    >= 23900 psi
    @Strain 0.2 %,
    Temperature 212 °F
     >= 165 MPa
    @Strain 1 %,
    Temperature 200 °C
    >= 23900 psi
    @Strain 1 %,
    Temperature 392 °F
     >= 200 MPa
    @Strain 1 %,
    Temperature 100 °C
    >= 29000 psi
    @Strain 1 %,
    Temperature 212 °F
    Elongation at Break >= 40 %>= 40 %
    Reduction of Area >= 50 %>= 50 %
    Modulus of Elasticity 200 GPa29000 ksi
     165 GPa
    @Temperature 500 °C
    23900 ksi
    @Temperature 932 °F
     172 GPa
    @Temperature 400 °C
    24900 ksi
    @Temperature 752 °F
     172 GPa
    @Temperature 400 °C
    24900 ksi
    @Temperature 752 °F
     179 GPa
    @Temperature 300 °C
    26000 ksi
    @Temperature 572 °F
     186 GPa
    @Temperature 200 °C
    27000 ksi
    @Temperature 392 °F
     186 GPa
    @Temperature 200 °C
    27000 ksi
    @Temperature 392 °F
     194 GPa
    @Temperature 100 °C
    28100 ksi
    @Temperature 212 °F
     194 GPa
    @Temperature 100 °C
    28100 ksi
    @Temperature 212 °F
     
    Thermal PropertiesMetricEnglishComments
    CTE, linear  16.5 µm/m-°C
    @Temperature 30.0 - 100 °C
    9.17 µin/in-°F
    @Temperature 86.0 - 212 °F
     17.0 µm/m-°C
    @Temperature 30.0 - 200 °C
    9.44 µin/in-°F
    @Temperature 86.0 - 392 °F
     17.5 µm/m-°C
    @Temperature 30.0 - 300 °C
    9.72 µin/in-°F
    @Temperature 86.0 - 572 °F
     18.0 µm/m-°C
    @Temperature 30.0 - 500 °C
    10.0 µin/in-°F
    @Temperature 86.0 - 932 °F
     18.0 µm/m-°C
    @Temperature 30.0 - 400 °C
    10.0 µin/in-°F
    @Temperature 86.0 - 752 °F
     18.5 µm/m-°C
    @Temperature 30.0 - 600 °C
    10.3 µin/in-°F
    @Temperature 86.0 - 1110 °F
     18.5 µm/m-°C
    @Temperature 30.0 - 700 °C
    10.3 µin/in-°F
    @Temperature 86.0 - 1290 °F
    Specific Heat Capacity  0.485 J/g-°C
    @Temperature 20.0 °C
    0.116 BTU/lb-°F
    @Temperature 68.0 °F
     0.500 J/g-°C
    @Temperature 100 °C
    0.120 BTU/lb-°F
    @Temperature 212 °F
     0.515 J/g-°C
    @Temperature 200 °C
    0.123 BTU/lb-°F
    @Temperature 392 °F
     0.525 J/g-°C
    @Temperature 300 °C
    0.125 BTU/lb-°F
    @Temperature 572 °F
     0.540 J/g-°C
    @Temperature 400 °C
    0.129 BTU/lb-°F
    @Temperature 752 °F
     0.555 J/g-°C
    @Temperature 500 °C
    0.133 BTU/lb-°F
    @Temperature 932 °F
     0.575 J/g-°C
    @Temperature 600 °C
    0.137 BTU/lb-°F
    @Temperature 1110 °F
    Thermal Conductivity  14.0 W/m-K
    @Temperature 20.0 °C
    97.2 BTU-in/hr-ft²-°F
    @Temperature 68.0 °F
     15.0 W/m-K
    @Temperature 100 °C
    104 BTU-in/hr-ft²-°F
    @Temperature 212 °F
     17.0 W/m-K
    @Temperature 200 °C
    118 BTU-in/hr-ft²-°F
    @Temperature 392 °F
     18.0 W/m-K
    @Temperature 300 °C
    125 BTU-in/hr-ft²-°F
    @Temperature 572 °F
     20.0 W/m-K
    @Temperature 400 °C
    139 BTU-in/hr-ft²-°F
    @Temperature 752 °F
     21.0 W/m-K
    @Temperature 500 °C
    146 BTU-in/hr-ft²-°F
    @Temperature 932 °F
     23.0 W/m-K
    @Temperature 600 °C
    160 BTU-in/hr-ft²-°F
    @Temperature 1110 °F
     
    Component Elements PropertiesMetricEnglishComments
    Carbon, C <= 0.030 %<= 0.030 %
    Chromium, Cr 17.5 %17.5 %
    Iron, Fe 65.2 %65.2 %As Balance
    Manganese, Mn 1.7 %1.7 %
    Molybdenum, Mo 2.6 %2.6 %
    Nickel, Ni 12.5 %12.5 %
    Phosphorus, P <= 0.040 %<= 0.040 %
    Silicon, Si 0.40 %0.40 %
    Sulfur, S <= 0.025 %<= 0.025 %

    Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

    Users viewing this material also viewed the following:
    Sandvik 303-6RA11 Billet
    Crucible Steel MCU Martensitic Steel
    Industeel CLC 17.12.2 L 2% Mo Containing 18 Cr –10 Ni Austenitic Stainless Steel
    Industeel CLC 17.13.3 LN Nitrogen Containing 18Cr-10Ni-2Mo Austenitic Stainless Steel
    Industeel CLC 18.12.4 LN 3%Mo Austenitic Stainless Steel with Nitrogen Addition

    NSANDV144 / 19038

    Free Trade Publications, Click Here!
    Free Trade Publications, Click Here!

    Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

    The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.