MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Haynes Hastelloy® N, weld metal, aged 500 hours at 649°C (1200°F)
Categories: Metal; Nonferrous Metal; Nickel Alloy; Superalloy

Material Notes: Applications include containers for molten fluoride salts. Good oxidation resistance to hot fluoride salts at 705-870°C (1300-1600°F), good oxidation resistance in air.

Data provided by the manufacturer, Haynes International, Inc.

Key Words: UNS N10003, AMS 5607, AMS 5771
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 8.86 g/cc
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength, Ultimate 805 MPa
 570 MPa
@Temperature 649 °C
Elongation at Break 38.6 %in 25.4 mm
 26.5 %
@Temperature 649 °C
in 25.4 mm
Modulus of Elasticity 122 GPa
@Temperature 1049 °C
 136 GPa
@Temperature 1000 °C
 143 GPa
@Temperature 954 °C
 151 GPa
@Temperature 904 °C
 157 GPa
@Temperature 854 °C
 163 GPa
@Temperature 800 °C
 171 GPa
@Temperature 700 °C
 181 GPa
@Temperature 577 °C
 181 GPa
@Temperature 632 °C
 187 GPa
@Temperature 500 °C
 192 GPa
@Temperature 410 °C
 202 GPa
@Temperature 221 °C
 219 GPa
@Temperature 14.0 °C
 
Electrical PropertiesOriginal ValueComments
Electrical Resistivity 0.000120 ohm-cmRT
 0.000124 ohm-cm
@Temperature 815 °C
 0.000126 ohm-cm
@Temperature 705 °C
 
Thermal PropertiesOriginal ValueComments
CTE, linear 12.3 µm/m-°C
@Temperature 21.0 - 316 °C
 12.7 µm/m-°C
@Temperature 21.0 - 427 °C
 13.4 µm/m-°C
@Temperature 21.0 - 538 °C
 14.0 µm/m-°C
@Temperature 21.0 - 649 °C
 14.7 µm/m-°C
@Temperature 21.0 - 760 °C
 15.3 µm/m-°C
@Temperature 21.0 - 871 °C
 15.8 µm/m-°C
@Temperature 21.0 - 982 °C
Specific Heat Capacity 0.419 J/g-°C
@Temperature 100 °C
 0.440 J/g-°C
@Temperature 200 °C
 0.456 J/g-°C
@Temperature 300 °C
 0.469 J/g-°C
@Temperature 400 °C
 0.477 J/g-°C
@Temperature 480 °C
 0.485 J/g-°C
@Temperature 540 °C
 0.523 J/g-°C
@Temperature 570 °C
 0.565 J/g-°C
@Temperature 590 °C
 0.578 J/g-°C
@Temperature 680 °C
 0.578 J/g-°C
@Temperature 700 °C
 0.582 J/g-°C
@Temperature 660 °C
 0.586 J/g-°C
@Temperature 620 °C
Thermal Conductivity 11.5 W/m-KRT
 13.1 W/m-K
@Temperature 100 °C
 13.1 W/m-K
@Temperature 200 °C
 14.4 W/m-K
@Temperature 300 °C
 16.5 W/m-K
@Temperature 400 °C
 18.0 W/m-K
@Temperature 500 °C
 20.3 W/m-K
@Temperature 600 °C
 23.6 W/m-K
@Temperature 700 °C
Melting Point 1300 - 1400 °C
Solidus 1300 °C
Liquidus 1400 °C
 
Component Elements PropertiesOriginal ValueComments
Al + Ti <= 0.50 %
Carbon, C <= 0.080 %
Chromium, Cr 7.0 %
Cobalt, Co <= 0.20 %
Copper, Cu <= 0.35 %
Iron, Fe <= 5.0 %
Manganese, Mn <= 0.80 %
Molybdenum, Mo 16 %
Nickel, Ni 71 %
Silicon, Si <= 1.0 %
Tungsten, W <= 0.50 %

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Haynes Hastelloy® D-205 Corrosion Resistant Alloy
Haynes Hastelloy® N, 1.6 mm sheet, heat treated at 1175°C, rapid air cooled
ATI Allvac® Nickelvac® H-X Nickel Superalloy, Heat Treatment: 1177°C (2150°F) Anneal
H.C. Starck Amperit® 529.074 Tungsten Carbide - Hastelloy C 85-15 (NiMoCrFeCo)
H.C. Starck Amperit® 529.053 Tungsten Carbide - Hastelloy C 85-15 (NiMoCrFeCo)

NHANBC / 16877

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.