MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

(Viewing data as-entered. Click here to return)
Solvay CYCOM® 5250-4 BMI Prepreg System with G30-500-3K-70PW Woven Carbon Fiber
Categories: Polymer; Thermoset; Bismaleimide (BMI); Carbon Fiber/Thermoset Composite

Material Notes: 58 Volume % G30-500-3K-70PW.

CYCOM® 5250-4 is a 350°F to 400°F (177°C to 204°C) curing bismaleimide resin with a service temperature range of -75°F to 400°F (-59°C to 204°C). CYCOM 5250-4 is specifically formulated for use in primary aircraft structures. In addition, a variety of secondary structural components can take advantage of the increased performance from using high-strain carbon fibers and the improved damage-resistance this system provides. CYCOM 5250-4 is available with either carbon fiber or glass fiber reinforcement in unidirectional tape, woven broadgood and roving forms.

Features & Benefits:

  • Short-term service temperature up to 450°F (232°C)
  • Superior hot/wet properties at 220°F to 375°F (104°C to 190°C)
  • Excellent toughness
  • Void-free laminates
  • High temperature resistance
  • Low thermal conductivity
  • Versatile cure
  • Excellent compression strength properties after impact
  • Shop life greater than 28 days at room temperature
  • Fluid/solvent resistant
Suggested Applications: Primary and secondary aircraft structure including:
  • Engine nacelles
  • Fuselage skins and stiffeners
  • Wing and stabilizer spars and skins
  • Other critical load-bearing components
Mechanical properties are reported for standard cure + standard post-cure

Information provided by Cytec, subsequently acquired by Solvay.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Density 1.25 g/ccNeat Resin; QC-PT-55
Volatiles 2.0 %
Water Absorption 1.3 %
@Temperature 149 °C
As Tested (Wet)
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength 135000 psi
@Temperature 24.0 °C
Warp (0°), G30-500-3K-70PW; ASTM D3039
Tensile Modulus 69.0 GPa
@Temperature 24.0 °C
Warp (0°), G30-500-3K-70PW
Compressive Strength 179 MPa
@Temperature 177 °C
Open Hole, [(+/-45),(0/90)], G30-500-3K-70PW
 230 MPa
@Temperature 149 °C
Open Hole, [(+/-45),(0/90)], G30-500-3K-70PW, wet
 262 MPa
@Temperature 121 °C
Open Hole, [(+/-45),(0/90)], G30-500-3K-70PW
 302 MPa
@Temperature 24.0 °C
Open Hole, [(+/-45),(0/90)], G30-500-3K-70PW
 414 MPa
@Temperature 163 °C
Warp (0°), G30-500-3K-70PW, Wet
 827 MPa
@Temperature 163 °C
Warp (0°), G30-500-3K-70PW
 932 MPa
@Temperature 24.0 °C
Warp (0°), G30-500-3K-70PW
Compressive Modulus 61000 MPaWarp (0°), G300-500-3K-70PW
Shear Strength 5000 psi
@Temperature 163 °C
Compression Interlaminar Warp (0°), G30-500-3K-70PW, Wet
 5000 psi
@Temperature 177 °C
Short Beam Warp, G30-500-3K-70PW, wet
 6400 psi
@Temperature 177 °C
Short Beam Warp, G30-500-3K-70PW
 8100 psi
@Temperature 121 °C
Short Beam Warp, G30-500-3K-70PW
 9000 psi
@Temperature 24.0 °C
Compression Interlaminar Warp (0°), G30-500-3K-70PW
 9200 psi
@Temperature 24.0 °C
Short Beam Warp, G30-500-3K-70PW
 
Thermal PropertiesOriginal ValueComments
Maximum Service Temperature, Air 400 °FContinuous; depends on cure cycle
 450 °Fshort term; depends on cure cycle
Minimum Service Temperature, Air -75.0 °F
Glass Transition Temp, Tg 200 °CWet; QC-PT-22
 216 °CPost Cure: 177°C for 6 hrs
 249 °CPost Cure: 190°C for 6 hrs
 263 °CPost Cure: 210°C for 6 hrs
 282 °CPost Cure: 227°C for 6 hrs
 300 °CDry; QC-PT-22
 304 °CPost Cure: 243°C for 6 hrs
 
Processing PropertiesOriginal ValueComments
Processing Temperature 350 - 400 °FCure Temperature - Autoclave
Gel Time 65.0 min
@Temperature 177 °C
in nitrogen atmosphere; QC-TP-87
Shelf Life >= 1.00 Month
@Temperature 72.0 °C
 >= 3.00 Month
@Temperature 4.44 °C
 >= 12.0 Month
@Temperature -17.8 °C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Solvay CYCOM® 5250-4 BMI Prepreg System with AS4-3K-70PW Woven Carbon Fiber
Solvay CYCOM® 5250-4 BMI Prepreg System with G30-500-3K-8HS Woven Carbon Fiber
Solvay CYCOM® 5250-4 BMI Prepreg System with IM-7 Carbon Fiber
Solvay CYCOM® 5250-4 BMI Prepreg System with G40-800 Carbon Fiber
Solvay CYCOM® 5250-4 BMI Prepreg System with IM7-6K-5HS Woven Carbon Fiber

PCYTED133_5 / 192681

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.