Physical Properties | Metric | English | Comments |
---|
Density | 3.76 g/cc | 0.136 lb/in³ |
Open Porosity | 0.00 % | 0.00 % |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Rockwell HR45N | 75 | 75 |
Flexural Strength | 296 MPa | 42900 psi |
Compressive Strength | >= 1720 MPa | >= 249000 psi |
|
Electrical Properties | Metric | English | Comments |
---|
Volume Resistivity | 8.40e+10 ohm-cm @Temperature 500 °C | 8.40e+10 ohm-cm @Temperature 932 °F |
| 1.00e+12 ohm-cm @Temperature 300 °C | 1.00e+12 ohm-cm @Temperature 572 °F |
| >= 1.00e+14 ohm-cm @Temperature 25.0 °C | >= 1.00e+14 ohm-cm @Temperature 77.0 °F |
Dielectric Constant | 9.0 @Frequency 1e+8 Hz, Temperature 25.0 °C | 9.0 @Frequency 1e+8 Hz, Temperature 77.0 °F |
| 9.04 @Frequency 8.50e+9 Hz, Temperature 25.0 °C | 9.04 @Frequency 8.50e+9 Hz, Temperature 77.0 °F |
| 9.32 @Frequency 8.50e+9 Hz, Temperature 300 °C | 9.32 @Frequency 8.50e+9 Hz, Temperature 572 °F |
| 9.53 @Frequency 1e+7 Hz, Temperature 25.0 °C | 9.53 @Frequency 1e+7 Hz, Temperature 77.0 °F |
| 9.54 @Frequency 8.50e+9 Hz, Temperature 500 °C | 9.54 @Frequency 8.50e+9 Hz, Temperature 932 °F |
| 9.91 @Frequency 1e+7 Hz, Temperature 300 °C | 9.91 @Frequency 1e+7 Hz, Temperature 572 °F |
| 10.14 @Frequency 1e+7 Hz, Temperature 500 °C | 10.14 @Frequency 1e+7 Hz, Temperature 932 °F |
Dielectric Strength | 43.3 kV/mm | 1100 kV/in |
Dissipation Factor | 0.000040 @Frequency 1e+7 Hz, Temperature 25.0 °C | 0.000040 @Frequency 1e+7 Hz, Temperature 77.0 °F |
| 0.00016 @Frequency 1e+7 Hz, Temperature 300 °C | 0.00016 @Frequency 1e+7 Hz, Temperature 572 °F |
| 0.00030 @Frequency 1e+8 Hz, Temperature 25.0 °C | 0.00030 @Frequency 1e+8 Hz, Temperature 77.0 °F |
| 0.00040 @Frequency 8.50e+9 Hz, Temperature 300 °C | 0.00040 @Frequency 8.50e+9 Hz, Temperature 572 °F |
| 0.00045 @Frequency 8.50e+9 Hz, Temperature 25.0 °C | 0.00045 @Frequency 8.50e+9 Hz, Temperature 77.0 °F |
| 0.00052 @Frequency 1e+7 Hz, Temperature 500 °C | 0.00052 @Frequency 1e+7 Hz, Temperature 932 °F |
| 0.00072 @Frequency 8.50e+9 Hz, Temperature 500 °C | 0.00072 @Frequency 8.50e+9 Hz, Temperature 932 °F |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 6.90 µm/m-°C @Temperature 25.0 - 200 °C | 3.83 µin/in-°F @Temperature 77.0 - 392 °F |
| 7.80 µm/m-°C @Temperature 200 - 400 °C | 4.33 µin/in-°F @Temperature 392 - 752 °F |
| 8.50 µm/m-°C @Temperature 400 - 600 °C | 4.72 µin/in-°F @Temperature 752 - 1110 °F |
| 8.80 µm/m-°C @Temperature 600 - 800 °C | 4.89 µin/in-°F @Temperature 1110 - 1470 °F |
| 9.00 µm/m-°C @Temperature 800 - 1000 °C | 5.00 µin/in-°F @Temperature 1470 - 1830 °F |
Thermal Conductivity | 26.8 W/m-K | 186 BTU-in/hr-ft²-°F |
Maximum Service Temperature, Air | 1650 °C | 3000 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Al2O3 | <= 97.6 % | <= 97.6 % |
|
Descriptive Properties |
---|
Color | white |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.