Physical Properties | Metric | English | Comments |
---|
Density | 7.80 g/cc | 0.282 lb/in³ |
|
Mechanical Properties | Metric | English | Comments |
---|
Hardness, Brinell | 220 - 270 @Thickness 160 - 180 mm | 220 - 270 @Thickness 6.30 - 7.09 in |
| 240 - 280 @Thickness 100 - 160 mm | 240 - 280 @Thickness 3.94 - 6.30 in |
| 270 - 320 @Thickness 40.0 - 100 mm | 270 - 320 @Thickness 1.57 - 3.94 in |
| 300 - 350 @Thickness 25.0 - 40.0 mm | 300 - 350 @Thickness 0.984 - 1.57 in |
Tensile Strength | 750 - 900 MPa @Thickness 160 - 180 mm | 109000 - 131000 psi @Thickness 6.30 - 7.09 in |
| 800 - 950 MPa @Thickness 100 - 160 mm | 116000 - 138000 psi @Thickness 3.94 - 6.30 in |
| 900 - 1100 MPa @Thickness 40.0 - 100 mm | 131000 - 160000 psi @Thickness 1.57 - 3.94 in |
| 1000 - 1200 MPa @Thickness 25.0 - 40.0 mm | 145000 - 174000 psi @Thickness 0.984 - 1.57 in |
Tensile Strength, Yield | >= 500 MPa @Thickness 160 - 180 mm | >= 72500 psi @Thickness 6.30 - 7.09 in |
| >= 550 MPa @Thickness 100 - 160 mm | >= 79800 psi @Thickness 3.94 - 6.30 in |
| >= 650 MPa @Thickness 40.0 - 100 mm | >= 94300 psi @Thickness 1.57 - 3.94 in |
| >= 750 MPa @Thickness 25.0 - 40.0 mm | >= 109000 psi @Thickness 0.984 - 1.57 in |
Elongation at Break | 11 % @Thickness 25.0 - 40.0 mm | 11 % @Thickness 0.984 - 1.57 in |
| 12 % @Thickness 40.0 - 100 mm | 12 % @Thickness 1.57 - 3.94 in |
| 13 % @Thickness 100 - 160 mm | 13 % @Thickness 3.94 - 6.30 in |
| 14 % @Thickness 160 - 180 mm | 14 % @Thickness 6.30 - 7.09 in |
Reduction of Area | 45 % @Thickness 25.0 - 40.0 mm | 45 % @Thickness 0.984 - 1.57 in |
| 50 % @Thickness 40.0 - 100 mm | 50 % @Thickness 1.57 - 3.94 in |
| 50 % @Thickness 100 - 160 mm | 50 % @Thickness 3.94 - 6.30 in |
| 55 % @Thickness 160 - 180 mm | 55 % @Thickness 6.30 - 7.09 in |
Modulus of Elasticity | 210 GPa | 30500 ksi |
Poissons Ratio | 0.30 | 0.30 |
Shear Modulus | 80.0 GPa | 11600 ksi |
Impact Test | 35.0 J @Thickness 25.0 - 40.0 mm, Temperature 20.0 °C | 25.8 ft-lb @Thickness 0.984 - 1.57 in, Temperature 68.0 °F |
| 35.0 J @Thickness 40.0 - 100 mm, Temperature 20.0 °C | 25.8 ft-lb @Thickness 1.57 - 3.94 in, Temperature 68.0 °F |
| 35.0 J @Thickness 100 - 160 mm, Temperature 20.0 °C | 25.8 ft-lb @Thickness 3.94 - 6.30 in, Temperature 68.0 °F |
| 35.0 J @Thickness 160 - 180 mm, Temperature 20.0 °C | 25.8 ft-lb @Thickness 6.30 - 7.09 in, Temperature 68.0 °F |
|
Electrical Properties | Metric | English | Comments |
---|
Electrical Resistivity | 0.00000200 - 0.00000250 ohm-cm | 0.00000200 - 0.00000250 ohm-cm |
|
Thermal Properties | Metric | English | Comments |
---|
CTE, linear | 12.0 µm/m-°C @Temperature 20.0 - 300 °C | 6.67 µin/in-°F @Temperature 68.0 - 572 °F |
Specific Heat Capacity | 0.460 - 0.480 J/g-°C @Temperature 50.0 - 100 °C | 0.110 - 0.115 BTU/lb-°F @Temperature 122 - 212 °F |
Thermal Conductivity | 40.0 - 45.0 W/m-K | 278 - 312 BTU-in/hr-ft²-°F |
Transformation Temperature | 320 °C | 608 °F |
| 740 °C | 1360 °F |
| 770 °C | 1420 °F |
|
Component Elements Properties | Metric | English | Comments |
---|
Carbon, C | 0.41 - 0.45 % | 0.41 - 0.45 % |
Chromium, Cr | 1.0 - 1.2 % | 1.0 - 1.2 % |
Iron, Fe | 96.57 - 97.35 % | 96.57 - 97.35 % |
Manganese, Mn | 0.65 - 0.80 % | 0.65 - 0.80 % |
Molybdenum, Mo | 0.22 - 0.28 % | 0.22 - 0.28 % |
Nickel, Ni | 0.15 - 0.30 % | 0.15 - 0.30 % |
Phosphorus, P | <= 0.025 % | <= 0.025 % |
Silicon, Si | 0.20 - 0.35 % | 0.20 - 0.35 % |
Sulfur, S | 0.020 - 0.030 % | 0.020 - 0.030 % |
|
Descriptive Properties |
---|
Weldability | CEV 0.92max |
| Pcm 0.6max |
Some of the values displayed above may have been converted from their original units and/or rounded in order to
display the information in a consistent format. Users requiring more precise data for scientific or engineering
calculations can click on the property value to see the original value as well as raw conversions to equivalent units.
We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding
error. We also ask that you refer to MatWeb's
terms of use regarding this information.
Click here to view
all the property values for this datasheet as they were originally entered into MatWeb.