MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

(Viewing data as-entered. Click here to return)
SEKISUI SPI KYDEX® T-IM Thermoplastic Compound, Injection Molding
Categories: Polymer; Thermoplastic

Material Notes: KYDEX® T-IM is a high performance injection molding compound with integral color engineered with the same properties as KYDEX® T thermoplastic sheet including flame resistance, impact resistance, and chemical resistance.

KYDEX® T-IM is designed for injection-molded parts adjacent to KYDEX® thermoplastic sheet parts. This solution is intended to minimize the visual variation between injection molded and thermoformed parts. It meets 12 and 60-second vertical burn requirements outlined in Federal Aviation Regulations (FAR) 25.853 paragraph (a). it is available in a wide range of aesthetic choices and Underwriter’s Laboratories, Inc.® recognized Std 94 V-0, 5V.

Suggested Application:

  • Aircraft Interiors
  • Equipment Housings
  • Kiosk Housings
  • Medical Products
Features:
  • Meets the vertical burn requirements of FAR 25.853 paragraph (a) in all thicknesses and colors
  • Excellent processing characteristics
  • Available in endless integral colors through our custom color creation
  • Excellent bonding capability with KYDEX® Thermoplastic Sheet
  • Color matching coordination with KYDEX® Thermoplastic Sheet
  • Chemical resistant
  • Recognized by Underwriter’s Laboratories, Inc® for Std 94 V-0, 5V in all thicknesses (testing pending)

Information provided by SEKISUI KYDEX, LLC.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.34 g/ccASTM D792
Moisture Absorption 0.0500 %
@Time 86400 sec
ASTM D570
Melt Flow 2.40 g/10 min
@Load 2.16 kg,
Temperature 200 °C
 
Mechanical PropertiesOriginal ValueComments
Hardness, Rockwell R 105ASTM D785
Tensile Strength 47.4 MPaASTM D638
Tensile Modulus 2558 MPaASTM D638
Flexural Strength 68.5 MPaASTM D790
Flexural Modulus 2510 MPaASTM D790
Compressive Yield Strength 50.6 MPaASTM D695
Compressive Modulus 2969 MPaASTM D695
Bearing Yield Strength <= 202 MPaASTM D953
Poissons Ratio 0.409ASTM D638
Shear Strength 52.3 MPaASTM D732
Izod Impact, Notched 801 J/mASTM D256
Gardner Impact 55.4 JDrop Dart Impact, GE; ASTM D5420
 
Electrical PropertiesOriginal ValueComments
Dielectric Strength 17.7 kV/mmoil; ASTM D149
 
Thermal PropertiesOriginal ValueComments
CTE, linear 75.8 µm/m-°CASTM E831
Deflection Temperature at 1.8 MPa (264 psi) 68.7 °Cannealed; ASTM D648
Flammability, UL94 V-0
 
Descriptive Properties
Vertical BurnPass60 and 12 sec; FAR 25.853(a)(i) and FAR 25.853(a)(ii)

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

PSEKIS509 / 325249

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.