System Message
Advertise with MatWeb!
Data sheets for over
180,000
metals, plastics, ceramics, and composites.
HOME
•
SEARCH
•
TOOLS
•
SUPPLIERS
•
FOLDERS
•
ABOUT US
•
FAQ
•
LOG IN
Recently Viewed Materials (most recent at top)
Login
to see your most recently viewed materials here.
Or if you don't have an account with us yet, then
click here to register.
Searches:
Advanced
|
Category
|
Property
|
Metals
|
Trade Name
|
Manufacturer
|
Recently Viewed Materials
(Viewing data as-entered.
Click here
to return)
Envalior Pocan® BF 4130 XF 000000 PBT, 30% Glass Fiber
Categories:
Polymer
;
Thermoplastic
;
Polyester, TP
;
Polybutylene Terephthalate (PBT)
;
Polybutylene Terephthalate (PBT), Glass Fiber Filled, Flame Retardant
Material Notes:
PBT, 30% glass fibers, injection molding, flame retardant, improved flowability
Former Lanxess product line is now with Envalior.
Vendors:
No vendors are listed for this material. Please
click here
if you are a supplier and would like information on how to add your listing to this material.
Printer friendly version
Download as PDF
Download to Excel (requires Excel and Windows)
Export data to your CAD/FEA program
Add to Folder:
My Folder
Physical Properties
Original Value
Comments
Specific Gravity
1.62
g/cc
ISO 1183
Bulk Density
0.700
g/cc
ISO 60
Viscosity Number
62
cm³/g
ISO 1628-5
Linear Mold Shrinkage, Flow
0.0010
cm/cm
Post-shrinkage, 60x60x2; 120°C; 4 hour; ISO 294-4
0.0030
cm/cm
60x60x2; 250°C / WZ 80°C; 600 bar; ISO 294-4
Linear Mold Shrinkage, Transverse
0.0010
cm/cm
Post-shrinkage, 60x60x2; 120°C; 4 hour; ISO 294-4
0.0080
cm/cm
60x60x2; 250°C / WZ 80°C; 600 bar; ISO 294-4
Melt Flow
17
g/10 min
@Load 2.16 kg,
Temperature 260 °C
ISO 1133-1
Mechanical Properties
Original Value
Comments
Ball Indentation Hardness
160
MPa
ISO 2039-1
Tensile Strength at Break
130
MPa
ISO 527-1, -2; 5 mm/min
Elongation at Break
2.2 %
ISO 527-1, -2; 5 mm/min
Tensile Modulus
10500
MPa
ISO 527-1, -2; 1 mm/min
Flexural Strength
200
MPa
@Strain 2.6 %
2 mm/min; ISO 178-A
Flexural Modulus
10000
MPa
2 mm/min; ISO 178-A
Izod Impact, Notched (ISO)
<=
10.0
kJ/m²
@Temperature 23.0 °C
ISO 180-1A
<=
10.0
kJ/m²
@Temperature -30.0 °C
ISO 180-1A
Izod Impact, Unnotched (ISO)
50.0
kJ/m²
@Temperature -30.0 °C
ISO 180-1U
55.0
kJ/m²
@Temperature 23.0 °C
ISO 180-1U
Charpy Impact Unnotched
50.0
kJ/m²
@Temperature -30.0 °C
ISO 179-1eU
55.0
kJ/m²
@Temperature 23.0 °C
ISO 179-1eU
Charpy Impact, Notched
<=
10.0
kJ/m²
@Temperature 23.0 °C
ISO 179-1eA
<=
10.0
kJ/m²
@Temperature -30.0 °C
ISO 179-1eA
Electrical Properties
Original Value
Comments
Comparative Tracking Index
200
V
d.a.m.; Solution A; IEC 60112
Thermal Properties
Original Value
Comments
CTE, linear, Parallel to Flow
20.0
µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1, -2
CTE, linear, Transverse to Flow
90.0
µm/m-°C
@Temperature 23.0 - 55.0 °C
ISO 11359-1, -2
Melting Point
228
°C
10°C/min; ISO 11357-1, -3
Maximum Service Temperature, Air
215
°C
Resistance to heat - ball pressure test; IEC 60695-10-2
Deflection Temperature at 0.46 MPa (66 psi)
220
°C
ISO 75-1, -2
Deflection Temperature at 1.8 MPa (264 psi)
205
°C
ISO 75-1, -2
Vicat Softening Point
205
°C
@Load 5.10 kg
120°C/hour; ISO 306
Flammability, UL94
V-0
@Thickness 1.50 mm
V-0
@Thickness 0.750 mm
Glow Wire Ignition Temperature
775
°C
@Diameter 0.800 mm
IEC 60695-2-13
775
°C
@Diameter 1.50 mm
IEC 60695-2-13
775
°C
@Diameter 3.00 mm
IEC 60695-2-13
Glow Wire Flammability Index
960
°C
@Diameter 0.800 mm
IEC 60695-2-12
960
°C
@Diameter 1.50 mm
IEC 60695-2-12
960
°C
@Diameter 3.00 mm
IEC 60695-2-12
Processing Properties
Original Value
Comments
Melt Temperature
240
-
260
°C
250
°C
for test specimens; ISO 294
Mold Temperature
80.0
°C
for test specimens; ISO 294
80.0
-
100
°C
Drying Temperature
120
°C
Dry Time
4
-
8
hour
Moisture Content
0.00 - 0.020 %
residual; Karl Fischer Test
Descriptive Properties
ISO Short Name
ISO 7792-PBT, GFHR, 07-100, GF30; ISO 1043-PBT GF FR(17)
Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's
terms of use
regarding this information.
Click here
to go back to viewing the property data in MatWeb's normal format.
Users viewing this material also viewed the following:
Celanese Celanex® 6400-2 PBT, Mineral / Glass Reinforced
Envalior Durethan® AM 40 X H2.0 901510 Nylon 66, Glass Fiber/Mineral Reinforced
Envalior Pocan® AF 4130 000000 PBT, 30% Glass Fiber Reinforced
Envalior Pocan® B 4235 Z 000000 PBT, 30% Glass Fiber Reinforced
Evonik Trogamid® T-GF35 35% Glass Reinforced Amorphous Nylon
PLANX0659 / 133622
Subscribe to Premium Services
Searches:
Advanced
•
Composition
•
Property
•
Material Type
•
Manufacturer
•
Trade Name
•
UNS Number
Other Links:
Advertising
•
Submit Data
•
Database Licensing
•
Web Design & Hosting
•
Trade Publications
Supplier List
•
Unit Converter
•
Reference
•
Links
•
Help
•
Contact Us
•
Site Map
•
FAQ
•
Home
Follow @MatWeb
Please read our
License Agreement
regarding materials data and our
Privacy Policy
. Questions or comments about MatWeb? Please contact us at
webmaster@matweb.com
. We appreciate your input.
The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.