MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

DuPont Mobility and Materials Zytel® 444AHS BK152 PA66-I  (discontinued **)
Categories: Polymer; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Impact Grade

Material Notes: Toughened, Heat Stabilized, Polyamide 66

While this product line has been acquired by Celanese, this specific grade had been disconued while still a DuPont product so it is listed here as a discontinued DuPont product.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.11 g/cc0.0401 lb/in³DAM; ISO 1183
Water Absorption 1.3 %
@Time 86400 sec
1.3 %
@Time 24.0 hour
DAM; Sim. to ISO 62
 1.3 %
@Thickness 2.00 mm
1.3 %
@Thickness 0.0787 in
DAM; Sim. to ISO 62
Linear Mold Shrinkage, Flow 0.014 cm/cm0.014 in/inDAM; ISO 294-4, 2577
Linear Mold Shrinkage, Transverse 0.012 cm/cm0.012 in/inDAM; ISO 294-4, 2577
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength, Yield 40.0 MPa5800 psi50% RH; ISO 527-1/-2
 62.0 MPa8990 psiDAM; ISO 527-1/-2
Elongation at Break 25 %25 %DAM; ISO 527-1/-2
 >= 50 %>= 50 %50% RH; ISO 527-1/-2
Elongation at Yield 5.5 %5.5 %DAM; ISO 527-1/-2
 15 %15 %50% RH; ISO 527-1/-2
Tensile Modulus 1.10 GPa160 ksi50% RH; ISO 527-1/-2
 2.40 GPa348 ksiDAM; ISO 527-1/-2
Flexural Modulus 2.27 GPa329 ksiDAM; ISO 178
Poissons Ratio 0.380.38DAM; ISO 527-1/-2
 0.450.4550%RH; ISO 527-1/-2
Izod Impact, Unnotched (ISO)  10.0 kJ/m²
@Temperature -40.0 °C
4.76 ft-lb/in²
@Temperature -40.0 °F
DAM; ISO 180/1A
 16.0 kJ/m²
@Temperature 23.0 °C
7.61 ft-lb/in²
@Temperature 73.4 °F
DAM; ISO 180/1A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow 90.0 µm/m-°C50.0 µin/in-°FDAM; ISO 11359-1/-2
CTE, linear, Transverse to Flow 100 µm/m-°C55.6 µin/in-°FDAM; ISO 11359-1/-2
Melting Point 260 °C500 °F10°C/min; DAM; ISO 11357-1/-3
Deflection Temperature at 1.8 MPa (264 psi) 65.0 °C149 °FDAM; ISO 75-1/-2
Flame Spread <= 80.0 mm/min
@Thickness 1.00 mm
<= 3.15 in/min
@Thickness 0.0394 in
ISO 3795 (FMVSS 302)
 
Processing PropertiesMetricEnglishComments
Melt Temperature 280 - 300 °C536 - 572 °FInjection
 290 °C554 °FInjection Optimum
Mold Temperature 50.0 - 90.0 °C122 - 194 °FInjection
 70.0 °C158 °FInjection Optimum
Ejection Temperature 190 °C374 °FInjection
Drying Temperature 80.0 °C176 °FInjection
Dry Time 2.00 - 4.00 hour2.00 - 4.00 hourDehumidified Dryer; Injection
Moisture Content 0.20 %0.20 %Injection
Hold Pressure 50.0 - 100 MPa7250 - 14500 psiInjection
 
Descriptive Properties
Delivery formPellets
Drying RecommendedyesInjection
FMVSS ClassBISO 3795 (FMVSS 302)
Hold pressure time (s/mm)4Injection
Max. screw tangential speed (m/s)0.3Injection
Part Marking CodePA66-IISO 11469
ProcessingInjection Molding
Regional AvailabilityNorth America
 South and Central America
Resin IdentificationPA66-IISO 1043
Special characteristicsHeat stabilized or stable to heat

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Celanese Zytel® 105F BK010 PA66
Overview of materials for Nylon 66, Impact Grade
DuPont Mobility and Materials Zytel® 42A NC010 PA66
DuPont Mobility and Materials Zytel® 101L BKB009 PA66
Celanese Zytel® 70K20HSL BK284 PA66-RF20

PDSX5315 / 197955

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.