MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Ascend Performance Materials Vydyne® 75HB NT0679 Nylon 66, Extrusion Grade  (discontinued **)
Categories: Polymer; Film; Thermoplastic; Nylon (Polyamide PA); Nylon 66 (PA66); Nylon 66, Extruded; Nylon 66, Film

Material Notes: 75HB NT0679 is a PA66-based copolymer that features high melt strength with ideal shear thinning behavior, high tensile strength, ductility, and improved clarity making it ideal for blown and cast film applications. Having a melt temperature between PA6 and PA66, it is a preferred material of choice compared to physical blends of PA6 and PA66 due to the ability to process at lower temperatures and produce a homogenous film resulting in uniform melting behavior, high gloss, and clarity. 75HB also allows for improved process flexibility due to its slower crystallization rate versus PA66 homopolymers.

Information provided by Ascend Performance Materials.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Bulk Density 0.674 g/ccASTM D1895
Density 1.14 g/ccISO 1183
Moisture Absorption 0.100 %ASTM D6869
Viscosity Measurement 4.0 - 4.2Relative Viscosity - Sulfuric Acid; ISO 307
 165 - 195Relative Viscosity - Formic Acid; ASTM D789
 
Mechanical PropertiesOriginal ValueComments
Film Tensile Strength at Yield, MD 31.0 MPa
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Film Tensile Strength at Yield, TD 31.0 MPa
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Tensile Strength, Yield 78.0 MPaDry; ISO 527-2
Film Elongation at Break, MD 390 %
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Film Elongation at Break, TD 480 %
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Film Elongation at Yield, MD 6.5 %
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Film Elongation at Yield, TD 6.4 %
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Elongation at Break 170 %Dry; ISO 527-2
Flexural Strength 84.0 MPaDry; ISO 178
Secant Modulus, MD 0.601 GPa
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Secant Modulus, TD 0.558 GPa
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Izod Impact, Notched (ISO) 7.00 kJ/m²
@Temperature 23.0 °C
Dry; ISO 180
Elmendorf Tear Strength MD 51 g
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D1922
Elmendorf Tear Strength TD 110 g
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D1922
Dart Drop Test >= 2000 g
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D1709A
Film Tensile Strength at Break, MD 121 MPa
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
Film Tensile Strength at Break, TD 101 MPa
@Thickness 0.0380 mm
Cast Film, Conditioned; ASTM D882
 
Thermal PropertiesOriginal ValueComments
Melting Point 244 °CISO 11357-3
 
Processing PropertiesOriginal ValueComments
Processing Temperature 20.0 - 60.0 °CBlow Film Air Temperature
 265 - 285 °CCylinder - Extrusion
Die Temperature 270 - 295 °CExtrusion
 70.0 - 80.0 °C
@Time 0.000 - 14400 sec
Extrusion
Melt Temperature 244 °CExtrusion
Moisture Content 0.030 - 0.080 %Extrusion
 
Compliance PropertiesOriginal ValueComments
European Food 1935/2004 Yes
FDA Yes21CFR 177.1500
 
Descriptive Properties
Agency RatingsEU 10/2011
 EU 2023/2006
FeaturesGood Chemical Resistance
 Good Toughness
 Heat Stabilized
 High Melt Stability
 High Rigidity
 High Strength
Melt Pressure MPa3-17
Processing MethodBlown Film
 Cast Film
 Extrusion
 Profile extrusion
Screw DesignGP or Barrier
UsesFilm, Multilayer
 Film, Vacuum Bagging
 Industrial Applications
 Monofilaments
 Profiles
 Rods
 Sheet
 Tubing

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Ascend Performance Materials Vydyne® 840B Nylon 66, Extrusion Grade
Ascend Performance Materials Vydyne® 833F Nylon 66, Extrusion Grade
Ascend Performance Materials Vydyne® 833C Nylon 66, Extrusion Grade
Ascend Performance Materials Vydyne® 75HB NT0679 Nylon 66 Compounding Grade
Arkema Kynar® Film 302 PGM TR PVDF

PZASCE9767 / 220870

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.