MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
Celanese Zenite® 7145L WT010 LCP (Extended Tabular Temperature Data)
Categories: Polymer; Thermoplastic; Liquid Crystal Polymer (LCP); Liquid Crystal Polymer (LCP), 50% Glass Fiber Filled

Material Notes: Zenite® 7145L WT010 is a 45% glass reinforced, lubricated liquid crystal polymer resin with high stiffness and a heat deflection temperature of 295°C.

Celenese acquired the Zenite product line from DuPont in 2010.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 1.81 g/ccASTM D 792
Density 1.81 g/ccISO 1183
Filler Content 45 %
Water Absorption 0.10 %
@Thickness 3.20 mm
Water, tap 23°C,24h; ASTM D570
Linear Mold Shrinkage, Flow 0.00010 cm/cm
@Thickness 3.17 mm
ASTM D955
 0.00050 cm/cm
@Thickness 2.00 mm
ISO 294-4
 0.00070 cm/cm
@Thickness 15.7 mm
ASTM D955
Linear Mold Shrinkage, Transverse 0.0030 cm/cm
@Thickness 3.17 mm
ASTM D955
 0.0050 cm/cm
@Thickness 1.60 mm
ASTM D955
 0.0050 cm/cm
@Thickness 2.00 mm
ISO 294-4
 
Mechanical PropertiesOriginal ValueComments
Tensile Strength at Break 120 MPaISO 527
Tensile Strength, Ultimate 40.0 MPa
@Thickness 3.17 mm,
Temperature 150 °C
ASTM D638
 45.0 MPa
@Thickness 1.60 mm,
Temperature 150 °C
ASTM D638
 50.0 MPa
@Thickness 3.17 mm,
Temperature 120 °C
ASTM D638
 57.0 MPa
@Thickness 1.60 mm,
Temperature 120 °C
ASTM D638
 119 MPa
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D638
 130 MPa
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D638
 171 MPa
@Thickness 3.17 mm,
Temperature -40.0 °C
ASTM D638
 190 MPa
@Thickness 1.60 mm,
Temperature -40.0 °C
ASTM D638
Elongation at Break 0.90 %ISO 527
 0.90 %
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D638
 1.1 %
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D638
Tensile Modulus 18000 MPaISO 527
 9000 MPa
@Thickness 3.17 mm,
Temperature 150 °C
ASTM D638
 10300 MPa
@Thickness 1.60 mm,
Temperature 149 °C
ASTM D638
 15200 MPa
@Thickness 3.17 mm,
Temperature 120 °C
ASTM D638
 18600 MPa
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D638
 18600 MPa
@Thickness 1.60 mm,
Temperature 120 °C
ASTM D638
 21000 MPa
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D638
 22800 MPa
@Thickness 3.17 mm,
Temperature -40.0 °C
ASTM D638
 26000 MPa
@Thickness 1.60 mm,
Temperature -40.0 °C
ASTM D638
Flexural Strength 24.0 MPa
@Thickness 3.17 mm,
Temperature 250 °C
ASTM D790
 29.0 MPa
@Thickness 0.790 mm,
Temperature 250 °C
ASTM D790
 43.0 MPa
@Thickness 3.17 mm,
Temperature 200 °C
ASTM D790
 50.0 MPa
@Thickness 0.790 mm,
Temperature 200 °C
ASTM D790
 58.0 MPa
@Thickness 3.17 mm,
Temperature 150 °C
ASTM D790
 71.0 MPa
@Thickness 1.60 mm,
Temperature 150 °C
ASTM D790
 71.0 MPa
@Thickness 3.17 mm,
Temperature 120 °C
ASTM D790
 75.0 MPa
@Thickness 0.790 mm,
Temperature 150 °C
ASTM D790
 92.0 MPa
@Thickness 0.790 mm,
Temperature 120 °C
ASTM D790
 158 MPa
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D790
 195 MPa
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D790
 205 MPa
@Thickness 0.790 mm,
Temperature 23.0 °C
ASTM D790
 225 MPa
@Thickness 3.17 mm,
Temperature -40.0 °C
ASTM D790
 280 MPa
@Thickness 1.60 mm,
Temperature -40.0 °C
ASTM D790
 300 MPa
@Thickness 0.790 mm,
Temperature -40.0 °C
ASTM D790
Flexural Modulus 17800 MPa
@Temperature 23.0 °C
ISO 178
 6600 MPa
@Thickness 3.17 mm,
Temperature 250 °C
ASTM D790
 7600 MPa
@Thickness 1.60 mm,
Temperature 250 °C
ASTM D790
 8300 MPa
@Thickness 0.790 mm,
Temperature 250 °C
ASTM D790
 8300 MPa
@Thickness 3.17 mm,
Temperature 150 °C
ASTM D790
 8600 MPa
@Thickness 3.17 mm,
Temperature 200 °C
ASTM D790
 9000 MPa
@Thickness 1.60 mm,
Temperature 200 °C
ASTM D790
 9700 MPa
@Thickness 0.790 mm,
Temperature 200 °C
ASTM D790
 9700 MPa
@Thickness 3.17 mm,
Temperature 120 °C
ASTM D790
 11000 MPa
@Thickness 1.60 mm,
Temperature 150 °C
ASTM D790
 13800 MPa
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D790
 14500 MPa
@Thickness 0.790 mm,
Temperature 150 °C
ASTM D790
 16000 MPa
@Thickness 3.17 mm,
Temperature -40.0 °C
ASTM D790
 17200 MPa
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D790
 18600 MPa
@Thickness 1.60 mm,
Temperature -40.0 °C
ASTM D790
 20700 MPa
@Thickness 0.790 mm,
Temperature 23.0 °C
ASTM D790
 24100 MPa
@Thickness 0.790 mm,
Temperature -40.0 °C
ASTM D790
Izod Impact, Notched 0.600 J/cm
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D256
 0.900 J/cm
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D256
 1.90 J/cm
@Thickness 0.790 mm,
Temperature 23.0 °C
ASTM D256
Izod Impact, Unnotched 316 J/m
@Thickness 3.17 mm,
Temperature 23.0 °C
ASTM D4812
 400 J/m
@Thickness 0.790 mm,
Temperature 23.0 °C
ASTM D4812
 653 J/m
@Thickness 1.60 mm,
Temperature 23.0 °C
ASTM D4812
Izod Impact, Notched (ISO) 8.00 kJ/m²
@Temperature 23.0 °C
ISO 180/1A
Charpy Impact Unnotched 1.20 J/cm²
@Temperature -30.0 °C
ISO 179/1eU
 1.40 J/cm²
@Temperature 23.0 °C
ISO 179/1eU
Charpy Impact, Notched 0.800 J/cm²
@Temperature -30.0 °C
ISO 179/1eA
 0.800 J/cm²
@Temperature 23.0 °C
ISO 179/1eA
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 4.3
@Frequency 60 Hz,
Temperature 23.0 °C
3.2mm (0.125in); ASTM D 150
 4.3
@Frequency 1e+6 Hz,
Temperature 23.0 °C
3.2mm (0.125in); ASTM D 150
 4.6
@Frequency 1000 Hz,
Temperature 23.0 °C
3.2mm (0.125in); ASTM D 150
 5.2
@Frequency 1e+6 Hz,
Temperature 120 °C
3.2mm (0.125in); ASTM D 150
 5.3
@Frequency 1e+6 Hz,
Temperature 150 °C
3.2mm (0.125in); ASTM D 150
 5.3
@Frequency 1000 Hz,
Temperature 120 °C
3.2mm (0.125in); ASTM D 150
 5.3
@Frequency 1e+6 Hz,
Temperature 200 °C
3.2mm (0.125in); ASTM D 150
 5.4
@Frequency 1000 Hz,
Temperature 150 °C
3.2mm (0.125in); ASTM D 150
 5.5
@Frequency 1000 Hz,
Temperature 200 °C
3.2mm (0.125in); ASTM D 150
 5.6
@Frequency 60 Hz,
Temperature 200 °C
3.2mm (0.125in); ASTM D 150
Dielectric Strength 20.0 kV/mm
@Thickness 3.20 mm,
Temperature 120 °C
Short time; ASTM D149
 20.0 kV/mm
@Thickness 3.20 mm,
Temperature 150 °C
Short time; ASTM D149
 20.0 kV/mm
@Thickness 3.20 mm,
Temperature 200 °C
Short time; ASTM D149
 21.0 kV/mm
@Thickness 3.20 mm,
Temperature 23.0 °C
Short time; ASTM D149
 25.0 kV/mm
@Thickness 1.60 mm,
Temperature 150 °C
Short time; ASTM D149
 26.0 kV/mm
@Thickness 1.60 mm,
Temperature 200 °C
Short time; ASTM D149
 27.0 kV/mm
@Thickness 1.60 mm,
Temperature 23.0 °C
Short time; ASTM D149
 32.0 kV/mm
@Thickness 0.800 mm,
Temperature 200 °C
Short time; ASTM D149
 33.0 kV/mm
@Thickness 0.800 mm,
Temperature 150 °C
Short time; ASTM D149
 33.0 kV/mm
@Thickness 0.800 mm,
Temperature 120 °C
Short time; ASTM D149
 34.0 kV/mm
@Thickness 0.800 mm,
Temperature 23.0 °C
Short time; ASTM D149
Dissipation Factor 0.0080
@Frequency 1000 Hz,
Temperature 120 °C
3.2mm (0.125in); ASTM D 150
 0.0080
@Frequency 1e+6 Hz,
Temperature 200 °C
3.2mm (0.125in); ASTM D 150
 0.0090
@Frequency 1000 Hz,
Temperature 150 °C
3.2mm (0.125in); ASTM D 150
 0.012
@Frequency 1e+6 Hz,
Temperature 150 °C
3.2mm (0.125in); ASTM D 150
 0.013
@Frequency 1000 Hz,
Temperature 23.0 °C
3.2mm (0.125in); ASTM D 150
 0.014
@Frequency 60 Hz,
Temperature 23.0 °C
3.2mm (0.125in); ASTM D 150
 0.015
@Frequency 1000 Hz,
Temperature 200 °C
3.2mm (0.125in); ASTM D 150
 0.023
@Frequency 1e+6 Hz,
Temperature 120 °C
3.2mm (0.125in); ASTM D 150
 0.025
@Frequency 1e+6 Hz,
Temperature 23.0 °C
3.2mm (0.125in); ASTM D 150
 0.083
@Frequency 60 Hz,
Temperature 200 °C
3.2mm (0.125in); ASTM D 150
Comparative Tracking Index 175 - 249 VUL 746A
 
Thermal PropertiesOriginal ValueComments
CTE, linear 0.000 µm/m-°C
@Thickness 2.00 mm,
Temperature 160 - 260 °C
ISO 11359-1/-2
 3.00 µm/m-°C
@Thickness 4.00 mm,
Temperature 160 - 260 °C
ISO 11359-1/-2
 3.00 µm/m-°C
@Thickness 2.00 mm,
Temperature 55.0 - 160 °C
ISO 11359-1/-2
 3.00 µm/m-°C
@Thickness 2.00 mm,
Temperature -40.0 - 23.0 °C
ISO 11359-1/-2
 3.00 µm/m-°C
@Thickness 2.00 mm,
Temperature -40.0 - 260 °C
ISO 11359-1/-2
 4.00 µm/m-°C
@Thickness 4.00 mm,
Temperature -40.0 - 260 °C
ISO 11359-1/-2
 4.00 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
 4.00 µm/m-°C
@Thickness 4.00 mm,
Temperature -40.0 - 23.0 °C
ISO 11359-1/-2
 5.00 µm/m-°C
@Thickness 4.00 mm,
Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
 5.00 µm/m-°C
@Thickness 4.00 mm,
Temperature 55.0 - 160 °C
ISO 11359-1/-2
CTE, linear, Transverse to Flow 51.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
ISO 11359-1/-2; 4mm
 52.0 µm/m-°C
@Temperature -40.0 - 23.0 °C
ISO 11359-1/-2; 2mm
 72.0 µm/m-°C
@Temperature -40.0 - 260 °C
ISO 11359-1/-2; 2mm
 72.0 µm/m-°C
@Temperature -40.0 - 260 °C
ISO 11359-1/-2; 4mm
 60.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
 60.0 µm/m-°C
@Thickness 4.00 mm,
Temperature 23.0 - 55.0 °C
ISO 11359-1/-2
 76.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 55.0 - 160 °C
ISO 11359-1/-2
 76.0 µm/m-°C
@Thickness 4.00 mm,
Temperature 55.0 - 160 °C
ISO 11359-1/-2
 78.0 µm/m-°C
@Thickness 2.00 mm,
Temperature 160 - 260 °C
ISO 11359-1/-2
 85.0 µm/m-°C
@Thickness 4.00 mm,
Temperature 160 - 260 °C
ISO 11359-1/-2
Melting Point 352 °C10°C/min; ISO 11357-1/-3
 357 °CASTM D 3418
Deflection Temperature at 1.8 MPa (264 psi) 295 °CISO 75-1/-2
 295 °CASTM D 648
Glass Transition Temp, Tg 120 °CASTM D 3418
UL RTI, Electrical 240 °C
@Thickness 1.50 mm
UL 746B
 240 °C
@Thickness 3.00 mm
UL 746B
UL RTI, Mechanical with Impact 210 °C
@Thickness 1.50 mm
UL 746B
 210 °C
@Thickness 3.00 mm
UL 746B
UL RTI, Mechanical without Impact 240 °C
@Thickness 1.50 mm
UL 746B
 240 °C
@Thickness 3.00 mm
UL 746B
Flammability, UL94 V-0
@Thickness 1.50 mm
IEC 60695-11-10
 V-0
@Thickness 1.50 mm
UL94
 V-0
@Thickness 3.00 mm
IEC 60695-11-10
 V-0
@Thickness 3.00 mm
UL94
Oxygen Index 38.5 %
@Thickness 3.17 mm
ASTM D2863
 
Processing PropertiesOriginal ValueComments
Melt Temperature 365 °COptimum
 360 - 370 °C
Mold Temperature 80.0 °COptimum
 40.0 - 150 °C
Drying Temperature 150 °C
Dry Time 3 hourDehumidified Dryer
Moisture Content <= 0.010 %
 
Descriptive Properties
AdditiveLubricant
ColorCream
Drying RecommendedYes
FeaturesAppearance, Pleasing Surface
 Appearance, Pleasing Surface
 Arc Resistant
 Arc Resistant
 Aromatic
 Aromatic
 Chemical Resistance, Good
 Chemical Resistance, Good
 Dimensional Stability, Good
 Dimensional Stability, Good
 Flow, Good
 Flow, Good
 Heat Aging Resistance, Good
 Heat Aging Resistance, Good
 Lubricated
 Lubricated
 Moisture Absorption, Low
 Moisture Absorption, Low
 Platable
 Platable
FillerGlass fiber reinforcement
Flame Retardant - Halogen/Red Phosphorus FreeYes
FormsPellets
GenericLCP
Part Marking Code>LCP-GF45<ISO 11469
Polymer FamilyLCP
Polymer TypeLCP
ProcessingInjection Moldable
Processing MethodInjection Molding
Product CategoryElectrical Resins
 Flame Retardant Resins
 Glass Reinforced Resins
Region AvailableAmericas
 Asia/Pacific
 Europe
Resin IdentificationLCP-GF45ISO 1043
UsesAutomotive Applications
 Automotive Electronics
 Automotive, Under the Hood
 Communication Applications
 Computer Components
 Connectors
 Electrical/Electronic Applications
 Parts, Engineering
 Parts, Thin-walled
 Printer Parts

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Celanese Zenite® 5145L BK010 LCP
Avient Therma-Tech™ LC-6000 TC Liquid Crystal Polymer (LCP)
Celanese ZENITE 6130L LCP, 30% Glass Reinforced
Celanese Zenite® 6635 BK010 LCP
Celanese Zenite® 7130 BK010 LCP (Extended Tabular Temperature Data)

PHCQ543b / 89630

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.