MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

3M Dyneon™ 1502 PTFE Powder  (discontinued **)
Categories: Polymer; Thermoplastic; Fluoropolymer; Polytetrafluoroethylene (PTFE); Polytetrafluoroethylene (PTFE), Molded

Material Notes: Type VI PTFE. The unique properties of polytetrafluoroethylene (PTFE) makes it an indispensable material for modern industry. PTFE offers the following exceptional characteristics:
  • Inert to a wide range of aggressive chemical agents
  • Ultra-low friction coefficient
  • Continuous service temperature range from cryogenic -330°F to 500°F
  • Extremely resistant to embrittlement, aging or weathering

PTFE has rapidly become the material choice where low friction, high durability, excellent thermal resistance and chemical inertness characteristics are required.

Data provided by Dyneon.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 2.16 g/cc0.0780 lb/in³Sintered moldings; ASTM D4894/D4895
Apparent Bulk Density 0.720 g/cc0.0260 lb/in³DIN 53 466
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 5353Sintered molding, DIN 53 505
Tensile Strength, Ultimate 30.0 MPa
@Thickness 2.00 mm
4350 psi
@Thickness 0.0787 in
Sintered moldings; ASTM D4894/4895
Elongation at Break 450 %450 %Sintered Molding; ASTM D4894
Tensile Modulus 0.600 GPa87.0 ksiSintered Molding, DIN 53457
 
Electrical PropertiesMetricEnglishComments
Electrical Resistivity 1.00e+14 ohm-cm1.00e+14 ohm-cmIEC 60093
Surface Resistance 1.00e+17 ohm1.00e+17 ohmIEC 60093
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  120 µm/m-°C
@Temperature 30.0 - 100 °C
66.7 µin/in-°F
@Temperature 86.0 - 212 °F
 140 µm/m-°C
@Temperature 30.0 - 200 °C
77.8 µin/in-°F
@Temperature 86.0 - 392 °F
 170 µm/m-°C
@Temperature 30.0 - 300 °C
94.4 µin/in-°F
@Temperature 86.0 - 572 °F
Thermal Conductivity 0.350 W/m-K2.43 BTU-in/hr-ft²-°FDIN 52 612
Maximum Service Temperature, Air 260 °C500 °FContinuous Service Temp
Minimum Service Temperature, Air -200 °C-328 °FContinuous Service Temp

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
Chemours Teflon® PTFE 7C Granular Molding Powder
Chemours Teflon® PTFE 7A Granular Molding Powder
3M Dyneon™ TFM™ 1700 Modified PTFE Powder
3M Dyneon™ TF 5050Z PTFE
3M Dyneon™ TF 2025Z PTFE Fine Powder

PDYM14 / 34659

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.