MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Multibase Multi-Pro® 3019 CXUW High Gloss 30% TiO2 Filler Content Polypropylene
Categories: Polymer; Thermoplastic; Polypropylene (PP); Polypropylene, Mineral Reinforced

Material Notes: Multi-Pro 3019 CXUW is a mineral reinforced polypropylene compound exhibiting high stiffness and impact characteristics. This material was specially formulated with UV stabilization for outdoor applications, and is particularly suited for injection molding of lawn furniture.

Data provided by Multibase.

Key Words: PP
Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 1.14 g/cc0.0412 lb/in³ASTM D792-91
Linear Mold Shrinkage 0.010 cm/cm0.010 in/inASTM D955-89
Melt Flow 19 g/10 min19 g/10 min(Condition L) ASTM D-1238-94a
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 737310 sec; ASTM D-2240-95
Tensile Strength, Ultimate 26.9 MPa3900 psiASTM D638-95
Elongation at Break 90 %90 %ASTM D638-95
Flexural Modulus 1.862 GPa270.1 ksiSecant 20% max load; ASTM D-790-95
Izod Impact, Notched 0.480 J/cm0.899 ft-lb/inASTM D256-93a
Gardner Impact 10.2 J7.52 ft-lbASTM D5420-93
 
Thermal PropertiesMetricEnglishComments
Deflection Temperature at 0.46 MPa (66 psi) 96.0 °C205 °FASTM D648-95
Deflection Temperature at 1.8 MPa (264 psi) 60.0 °C140 °FASTM D648-95
 
Optical PropertiesMetricEnglishComments
Gloss 70 %70 %ASTM D2457-90

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

Users viewing this material also viewed the following:
MarkeTech Rutile (TiO2) Fiber Optic Crystal
Titanium Dioxide, Brookite
Titanium (IV) Oxide, TiO2
Momentive Performance Materials HPC Boron Nitride (BN)/TiO2 Water Based Coating
H.C. Starck Amperit® 745.8 Aluminum Oxide-Titanium Oxide 60-40 (Al2O3-TiO2)

PLA261 / 49658

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.