MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Elmet Technologies

3M Dyneon™ PFA 6503 A EPC Perfluoroalkoxy Fluorothermoplastic  (discontinued **)
Categories: Polymer; Thermoplastic; Fluoropolymer; Perfluoroalkoxy (PFA)

Material Notes: Dyneon PFA 6503 A EPC is a fluorothermoplastic powder for powder coating applications, and is designed for thin film applications where target film thickness is 25-40 micrometers per pass.
  • non-stick surfaces
  • chemical vessel and tank liners
  • electrical insulation
  • low friction applications

Information provided by Dyneon, A 3M Company

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 2.15 g/cc2.15 g/ccASTM D792
Bulk Density 0.800 g/cc0.0289 lb/in³DIN 53466
Particle Size 25 µm25 µmmedian
Melt Index of Compound 3.0 g/10 min
@Load 5.00 kg,
Temperature 372 °C
3.0 g/10 min
@Load 11.0 lb,
Temperature 702 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore D 6060ASTM D2240
Tensile Strength at Break 30.0 MPa4350 psiASTM D638
Elongation at Break 380 %380 %ASTM D638
Flexural Modulus 0.550 GPa79.8 ksiASTM D790
 
Thermal PropertiesMetricEnglishComments
Melting Point 308 °C586 °FASTM D4591
Oxygen Index >= 95 %>= 95 %ASTM D2863
 
Descriptive Properties
FormAgglomerate

**
Materials flagged as discontinued () are no longer part of the manufacturer’s standard product line according to our latest information. These materials may be available by special order, in distribution inventory, or reinstated as an active product. Data sheets from materials that are no longer available remain in MatWeb to assist users in finding replacement materials.

Users of our Advanced Search (registration required) may exclude discontinued materials from search results.

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PDYNE016 / 34824

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.