MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Specialty Compounds RTP Company

SABIC NORYL™ Resin GFN1 Polyphenylene Ether + PS (PPE+PS) (Asia)
Categories: Polymer; Thermoplastic; Polystyrene (PS); Polystyrene + Polyphenylene Ether, Unreinforced

Material Notes: NORYL™ GFN1 resin is a 10% glass reinforced blend of polyphenylene ether (PPE) + high impact polystyrene (HIPS). This general-purpose injection moldable grade exhibits very low moisture absorption, high strength, hydrolytic stability, Low warpage, low specific gravity, and dimensional stability. NORYL GFN1 carries a UL746C outdoor suitability rating of F1 and is an excellent candidate for a variety of indoor and outdoor applications including construction, electrical components + displays, lawn and garden equipment. *See NORYL GFN1F resin for FDA food compliant / NSF version.

Features: Hydrolytic Stability,Good Stiffness,Low Warpage,Structural

Information provided by SABIC

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Specific Gravity 1.17 g/cc1.17 g/ccASTM D792
Density 1.17 g/cc0.0423 lb/in³ISO 1183
Moisture Absorption 0.0200 %0.0200 %Injection Molding
 0.0400 %0.0400 %23°C / 50% RH; ISO 62
Water Absorption at Saturation 0.12 %0.12 %ISO 62-1
Viscosity 4.0 cP
@Load 5.00 kg,
Temperature 280 °C
4.0 cP
@Load 11.0 lb,
Temperature 536 °F
MVR cc/10 min; ISO 1133
Linear Mold Shrinkage, Flow 0.0055 - 0.0066 cm/cm
@Thickness 3.20 mm
0.0055 - 0.0066 in/in
@Thickness 0.126 in
SABIC method
Melt Flow 4.0 g/10 min
@Load 5.00 kg,
Temperature 280 °C
4.0 g/10 min
@Load 11.0 lb,
Temperature 536 °F
ASTM D1238
 
Mechanical PropertiesMetricEnglishComments
Tensile Strength at Break 60.0 MPa8700 psi50 mm/min; ISO 527
 75.0 MPa10900 psi50 mm/min; ASTM D638
Tensile Strength, Yield 60.0 MPa8700 psi50 mm/min; ISO 527
 75.0 MPa10900 psi50 mm/min; ASTM D638
Elongation at Break 3.5 %3.5 %50 mm/min; ASTM D638
 4.5 %4.5 %50 mm/min; ISO 527
Elongation at Yield 3.5 %3.5 %50 mm/min; ASTM D638
 4.5 %4.5 %50 mm/min; ISO 527
Tensile Modulus 3.90 GPa566 ksi1 mm/min; ISO 527
 4.40 GPa638 ksi5 mm/min; ASTM D638
Flexural Strength 105 MPa15200 psiyld, 1.3 mm/min, 50 mm span; ASTM D790
 115 MPa16700 psiyield, 2 mm/min; ISO 178
Flexural Modulus 3.40 GPa493 ksi1.3 mm/min, 50 mm span; ASTM D790
 3.70 GPa537 ksi2 mm/min; ISO 178
Izod Impact Notched 84.0 J62.0 ft-lbASTM D256
 80.0 J
@Temperature -30.0 °C
59.0 ft-lb
@Temperature -22.0 °F
ASTM D256
Izod Impact, Unnotched 4.10 J/cm7.68 ft-lb/inASTM D4812
Izod Impact, Notched (ISO) 10.0 kJ/m²4.76 ft-lb/in²80*10*4; ISO 180/1A
 9.00 kJ/m²
@Temperature -30.0 °C
4.28 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1A
Izod Impact, Unnotched (ISO) 30.0 kJ/m²14.3 ft-lb/in²80*10*4; ISO 180/1U
 30.0 kJ/m²
@Temperature -30.0 °C
14.3 ft-lb/in²
@Temperature -22.0 °F
80*10*4; ISO 180/1U
Charpy Impact, Notched 0.800 J/cm²3.81 ft-lb/in²Edgew 80*10*4 sp=62mm; ISO 179/1eA
Dart Drop, Total Energy 20.0 J14.8 ft-lbASTM D3763
 
Electrical PropertiesMetricEnglishComments
Arc Resistance 60 - 120 sec60 - 120 secASTM D495
Comparative Tracking Index 175 - 250 V175 - 250 VUL 746A
Hot Wire Ignition, HWI  30 - 60 sec
@Thickness >=3.00 mm
30 - 60 sec
@Thickness >=0.118 in
UL 746A
 60 - 120 sec
@Thickness >=1.50 mm
60 - 120 sec
@Thickness >=0.0591 in
UL 746A
High Amp Arc Ignition, HAI  0.00 - 15 arcs
@Thickness >=3.00 mm
0.00 - 15 arcs
@Thickness >=0.118 in
UL 746A
 15 - 30 arcs
@Thickness >=1.50 mm
15 - 30 arcs
@Thickness >=0.0591 in
UL 746A
High Voltage Arc-Tracking Rate, HVTR >= 150 mm/min>= 5.91 in/minUL 746A
 
Thermal PropertiesMetricEnglishComments
CTE, linear, Parallel to Flow  38.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
21.1 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
 45.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
25.0 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
CTE, linear, Transverse to Flow  82.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
45.6 µin/in-°F
@Temperature -40.0 - 104 °F
ASTM E831
 85.0 µm/m-°C
@Temperature -40.0 - 40.0 °C
47.2 µin/in-°F
@Temperature -40.0 - 104 °F
ISO 11359-2
Deflection Temperature at 0.46 MPa (66 psi) 135 °C
@Thickness 3.20 mm
275 °F
@Thickness 0.126 in
unannealed; ASTM D648
Deflection Temperature at 1.8 MPa (264 psi) 129 °C264 °FFlatw 80*10*4 sp=64mm; ISO 75/Af
 130 °C
@Thickness 3.20 mm
266 °F
@Thickness 0.126 in
unannealed; ASTM D648
Vicat Softening Point 138 °C280 °FRate B/50; ASTM D1525
 138 °C280 °FRate B/50; ISO 306
 140 °C284 °FRate B/120; ISO 306
UL RTI, Electrical 90.0 °C194 °FUL 746B
UL RTI, Mechanical with Impact 90.0 °C194 °FUL 746B
UL RTI, Mechanical without Impact 90.0 °C194 °FUL 746B
Flammability, UL94 HB
@Thickness >=1.50 mm
HB
@Thickness >=0.0591 in
UL 94
 
Processing PropertiesMetricEnglishComments
Nozzle Temperature 295 - 315 °C563 - 599 °F
Zone 2 270 - 310 °C518 - 590 °F
Zone 3 280 - 315 °C536 - 599 °F
Melt Temperature 295 - 315 °C563 - 599 °FInjection Molding
Mold Temperature 75.0 - 105 °C167 - 221 °F
Drying Temperature 105 - 110 °C221 - 230 °FInjection Molding
Dry Time 3.00 - 4.00 hour3.00 - 4.00 hourInjection Molding
 8.00 hour8.00 hourCumulative; Injection Molding
Back Pressure 0.300 - 0.700 MPa43.5 - 102 psi
Shot Size 30 - 70 %30 - 70 %
Screw Speed 20 - 100 rpm20 - 100 rpm
 
Descriptive Properties
UV-light, water exposure/immersionF1UL 746C

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PSABH82305 / 290252

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.