MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Rulon Bearings

(Viewing data as-entered. Click here to return)
A. Schulman BMC 1901 Mineral Filled Alkyd
Categories: Polymer; Thermoset; Filled/Reinforced Thermoset; Polyester, TS; Alkyd (Polyester), Molded, Mineral Filler

Material Notes: BMC 1901 molding compound is a mineral filled, glass-fiber-reinforced alkyd compound suitable for compression transfer molding. It is a general purpose with medium impact strength and good overall electrical properties.

Typical applications include switch components, relay bases, stack insulator s and as a formable insulating putty for motor construction and repair.

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesOriginal ValueComments
Specific Gravity 2.21 g/cc
Water Absorption 0.28 %24 hours, 23°C
Linear Mold Shrinkage 0.0030 - 0.0060 cm/cm
 
Mechanical PropertiesOriginal ValueComments
Hardness, Barcol 60 - 80
Flexural Strength 15000 - 20000 psi
Compressive Strength 22000 - 26000 psi
Izod Impact, Notched 2.00 - 4.00 ft-lb/in
 
Electrical PropertiesOriginal ValueComments
Dielectric Constant 7.3
@Frequency 60 Hz
Dielectric Strength 325 V/milShort Time
Dissipation Factor 0.40
@Frequency 60 Hz
Arc Resistance >= 180 sec
Comparative Tracking Index >= 600 V
 
Thermal PropertiesOriginal ValueComments
Deflection Temperature at 1.8 MPa (264 psi) >= 500 °F
Flammability, UL94 HB
@Thickness 6.35 mm
 HB
@Thickness 3.17 mm
 HB
@Thickness 1.59 mm
 
Processing PropertiesOriginal ValueComments
Mold Temperature 280 - 330 °F

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to go back to viewing the property data in MatWeb's normal format.

Users viewing this material also viewed the following:
Overview of materials for Thermoset Polyester Glass Filled BMC
Plenco 08133 Polyester BMC, Compression Molded
Raschig Group RALUPOL® 2100 UP Polyester
Overview of materials for Silicone Rubber
Overview of materials for PVC, Molded

PBMC056 / 27239

Aluminum Castings

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at info@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2025 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.