MatWeb - Material Property Data Advertise with MatWeb!     Register Now
Data sheets for over 180,000 metals, plastics, ceramics, and composites.
MatWeb - Material Property Data HOME  •   SEARCH  •   TOOLS  •   SUPPLIERS  •   FOLDERS  •   ABOUT US  •   FAQ  •   LOG IN    
Recently Viewed Materials (most recent at top)  

Login to see your most recently viewed materials here.

Or if you don't have an account with us yet, then click here to register.

  Searches:   Advanced  | Category  | Property  | Metals  | Trade Name  | Manufacturer  | Recently Viewed Materials
  

Master Bond adhesives

Teknor Apex Sarlink® TPV 3190 Thermoplastic Vulcanizate
Categories: Polymer; Thermoplastic; Elastomer, TPE; Thermoplastic Vulcanizate Elastomer (TPV)

Material Notes: Notes: Sarlink TPV 3100 series are engineered materials designed primarily general purpose, automotive and industrial applications requiring a good balance of thermal, mechanical, and physical properties. Sarlink 3180, available in NAT and BLK, is a medium hardness, low density, multi-purpose thermoplastic vulcanizate that can be processed by injection molding, blow molding or extrusion for applications such as grips, seals, gaskets, profiles, hose & tubes, bellows, and other articles.

Availability: Africa & Middle East; Asia Pacific; Europe; Latin America; North America

Features: Chemical Resistant; Fatigue Resistant; General Purpose; Good Adhesion; Good Flexibility; Good Moldability; Good Processability; Good Surface Finish; Heat Aging Resistant; High Hardness; Low Density; Low Specific Gravity; Resilient; Weather Resistant

Uses: Automotive Applications; Automotive Exterior Parts; Automotive Interior Parts; Automotive Under the Hood; Blow Molding Applications; Gaskets; Industrial Applications; Profiles; Rubber Replacement; Seals; Sheets; Weatherstripping

RoHS Compliance: RoHS Compliant

Automotive Specifications: CHRYSLER MS-AR-80 Type D Color: Black; CHRYSLER MS-AR-80 Type D Color: Natural; Food WSD-M2D381-A1 Color: Black; GM QK 3526 Type 6 Color: Natural; GM QK 3526 Type 6 Color: Black; NISSAN Unspecified Color: Black; PSA Peugeot-Citroen B62 0300 version G Color: Black; RENAULT F.E.M. 03 20 007 Color: Black; VAG VW501 23 Color: Black

UL File Number: QMFZ2.E54709

Agency Ratings: UL 94

Form: Pellets

Processing Method: Extrusion; Injection Molding; Blow Molding

Information provided by Teknor Apex

Vendors: No vendors are listed for this material. Please click here if you are a supplier and would like information on how to add your listing to this material.
 
Physical PropertiesMetricEnglishComments
Density 0.940 g/cc0.0340 lb/in³ASTM D792
Viscosity 310 cP
@Shear Rate 206 1/s,
Temperature 200 °C
310 cP
@Shear Rate 206 1/s,
Temperature 392 °F
Shear, Capillary; ASTM D3835
 
Mechanical PropertiesMetricEnglishComments
Hardness, Shore A  89
@Time 5.00 sec
89
@Time 0.00139 hour
Extruded; ISO 868
 92
@Time 5.00 sec
92
@Time 0.00139 hour
Injection Molded; ISO 868
Tensile Strength 6.60 MPa957 psiAcross Flow; ISO 37
 10.0 MPa1450 psiFlow; ISO 37
 5.94 MPa
@Temperature 135 °C
861 psi
@Temperature 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
 6.27 MPa
@Temperature 150 °C
909 psi
@Temperature 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
Tensile Stress at Strain  12.1 MPa
@Strain 100 %
1750 psi
@Strain 100 %
Flow; ISO 37
 13.5 MPa
@Strain 100 %
1960 psi
@Strain 100 %
Across Flow; ISO 37
 14.7 MPa
@Strain 100 %,
Treatment Temp. 135 °C
2140 psi
@Strain 100 %,
Treatment Temp. 275 °F
Across Flow, Change in Air at 1000 hr; ISO 188
 15.0 MPa
@Strain 100 %,
Treatment Temp. 150 °C
2180 psi
@Strain 100 %,
Treatment Temp. 302 °F
Across Flow, Change in Air at 168 hr; ISO 188
Elongation at Break 380 %380 %Flow; ISO 37
 700 %700 %Across Flow; ISO 37
 595 %
@Treatment Temp. 135 °C,
Time 3.60e+6 sec
595 %
@Treatment Temp. 275 °F,
Time 1000 hour
Across Flow, Change in Air; ISO 188
 616 %
@Treatment Temp. 150 °C,
Time 605000 sec
616 %
@Treatment Temp. 302 °F,
Time 168 hour
Across Flow, Change in Air; ISO 188
Tear Strength 80.6 kN/m460 pliMethod Ba, Angle (Unnicked); ISO 34-1
Compression Set  48 %
@Temperature 22.8 °C,
Time 79200 sec
48 %
@Temperature 73.0 °F,
Time 22.0 hour
ISO 815
 61 %
@Temperature 70.0 °C,
Time 79200 sec
61 %
@Temperature 158 °F,
Time 22.0 hour
ISO 815
 75 %
@Temperature 125 °C,
Time 252000 sec
75 %
@Temperature 257 °F,
Time 70.0 hour
ISO 815
 
Processing PropertiesMetricEnglishComments
Processing Temperature 185 - 220 °C365 - 428 °FInjection, Melt
Rear Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Middle Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Front Barrel Temperature 180 - 215 °C356 - 419 °FInjection
Nozzle Temperature 187 - 220 °C369 - 428 °FInjection
Zone 1 180 - 200 °C356 - 392 °FExtrusion
Zone 2 180 - 205 °C356 - 401 °FExtrusion
Zone 3 187 - 210 °C369 - 410 °FExtrusion
Zone 4 187 - 210 °C369 - 410 °FExtrusion
Die Temperature 195 - 215 °C383 - 419 °FExtrusion
Mold Temperature 10.0 - 55.0 °C50.0 - 131 °FInjection
Drying Temperature 82.2 °C180 °F
Dry Time 3.00 hour3.00 hour
Back Pressure 0.100 - 1.00 MPa14.5 - 145 psiInjection
Screw Speed 100 - 200 rpm100 - 200 rpmInjection
 
Descriptive Properties
AppearanceBlack
 Natural Color
 Opaque

Some of the values displayed above may have been converted from their original units and/or rounded in order to display the information in a consistent format. Users requiring more precise data for scientific or engineering calculations can click on the property value to see the original value as well as raw conversions to equivalent units. We advise that you only use the original value or one of its raw conversions in your calculations to minimize rounding error. We also ask that you refer to MatWeb's terms of use regarding this information. Click here to view all the property values for this datasheet as they were originally entered into MatWeb.

PTEKNQ1145 / 237636

Please read our License Agreement regarding materials data and our Privacy Policy. Questions or comments about MatWeb? Please contact us at webmaster@matweb.com. We appreciate your input.

The contents of this web site, the MatWeb logo, and "MatWeb" are Copyright 1996-2024 by MatWeb, LLC. MatWeb is intended for personal, non-commercial use. The contents, results, and technical data from this site may not be reproduced either electronically, photographically or substantively without permission from MatWeb, LLC.